Dear Mates,

Thanks to all for your valuable feedback.
As per my request client provided the piping class document and the subject nozzles with flat face flange will be used with FF Gaskets. So the entire flat face need unpainted and shall be protected with rust prevention compound like MOLYKOTE. So we removed all the paint from the flat face with paint remover and thinner and applied rust prevention compound.

Thanks again.

On Thu, Feb 28, 2013 at 1:43 PM, Gerlof Oegema <Gerlof.Oegema@aurecongroup.com> wrote:
Hi,

It is always good practice to slightly paint the clamped area of flange face only with a red oxide paint to maximum DFT of 40 microns (with gramophone finish still visible) as to prevent corrosion of this clamped area while waiting to be installed.

Regards,
G. Oegema

 
DISCLAIMER
-----Original Message-----
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Praphulla Phirke
Sent: Thursday, February 28, 2013 11:36 AM
To: materials-welding@googlegroups.com
Cc: materials-welding@googlegroups.com
Subject: Re: [MW:16901] FLAT FACE FLANGE PAINTING

What is the test pressure ?

Better to remove the paint completely and You can use either neoprene or PTFE gaskets.

Praphulla
Sent from my iPhone

On 28-Feb-2013, at 14:05, Lalu r p <lalucpt@gmail.com> wrote:

> Dear sir
> Normally for flange faces we do not paint the surface to ensure the
> proper sealing.and it is normally machined for the gasket tightness.
>
> On 2/28/13, G Sreenivas Rao <gsrinivasg3@gmail.com> wrote:
>> Dear sir
>> In pressure vessel flat flange shall not be painted, this is for
>> gasket seating and if painted the are will not be giving seal
>> tightness. please ensure if the area is giving seal tightness then
>> can be left as it is.
>>
>> Regards
>> G.Sreenivas Rao
>>
>> On Wed, Feb 27, 2013 at 12:26 PM, Suresh Babu
>> <suresh75.babu@gmail.com>
>> wrote:
>>> Dear Experts,
>>>
>>> We have some flat face flanges in Pressure vessel. The pressure
>>> vessel manufacturer done the painting on the flat face up to the
>>> bolt hole and left the remaining face unpainted. I hope the entire
>>> flat face will leave as unpainted. I am trying to get info from
>>> client which type of Gasket they will use at site.
>>>
>>> Please put your suggestions.
>>>
>>> --
>>> Best Regards,
>>> Suresh Babu,
>>> suresh75.babu@gmail.com
>>>
>>> --
>>> To post to this group, send email to
>>> materials-welding@googlegroups.com
>>> To unsubscribe from this group, send email to
>>> materials-welding+unsubscribe@googlegroups.com
>>> For more options, visit this group's bolg at
>>> http://materials-welding.blogspot.com/
>>> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122
>>> 787&trk=anet_ug_hm
>>>
>>> The views expressed/exchnaged in this group are members personel
>>> views and meant for educational purposes only, Users must take their
>>> own decisions w.r.t. applicable code/standard/contract documents.
>>> ---
>>> You received this message because you are subscribed to the Google
>>> Groups "Materials & Welding" group.
>>> To unsubscribe from this group and stop receiving emails from it,
>>> send an email to materials-welding+unsubscribe@googlegroups.com.
>>> For more options, visit https://groups.google.com/groups/opt_out.
>>
>> --
>> To post to this group, send email to
>> materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=1227
>> 87&trk=anet_ug_hm
>>
>> The views expressed/exchnaged in this group are members personel
>> views and meant for educational purposes only, Users must take their
>> own decisions w.r.t. applicable code/standard/contract documents.
>> ---
>> You received this message because you are subscribed to the Google
>> Groups "Materials & Welding" group.
>> To unsubscribe from this group and stop receiving emails from it,
>> send an email to materials-welding+unsubscribe@googlegroups.com.
>> For more options, visit https://groups.google.com/groups/opt_out.
>
> --
> To post to this group, send email to
> materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=12278
> 7&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
> For more options, visit https://groups.google.com/groups/opt_out.
>
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.




--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.





--
Best Regards,
Suresh Babu,

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...