Skip to main content

RE: [MW:16868] Pitting Corrosion Resistance Failure in DSS

Dear Siddig,

 

Intelligent pig is not possible because these are process piping on the platform and the pipe range from 2" till 20 ".

 

 

Regards

 

Siva

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of siddig Abdelaziz
Sent: Monday, February 25, 2013 3:42 PM
To: materials - welding
Subject: RE: [MW:16864] Pitting Corrosion Resistance Failure in DSS
Importance: High

 

Dear all
good day , I recommended the the Intelligent pig  

Kindest regards,

Siddig Hamid Mohammed

 Pipe Line Repair  Section Head.

Sudanese Petroleum Pipelines Co. (SPPC)

one of Petrolines for Pipes & Engineering Work Holding Co.

T      +249 187 027223  IP Phone Ext. 7223

F      +249 183 027120

E   sdhamid@sppc-sd.com

W    www.sppc-sd.com

 ـــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــــ

M     +249-912221242

P Please don't print this email unless you really need to.

 


 


From: sivaselvam@kpoc.com.my
To: materials-welding@googlegroups.com
Subject: RE: [MW:16861] Pitting Corrosion Resistance Failure in DSS
Date: Mon, 25 Feb 2013 06:46:35 +0000

Dear Parag,

 

Sorry for the misunderstanding.

 

The corrosion I am referring  is the internal corrosion at weld joint, what NDT technique is suitable for this?

 

Regards

 

Siva

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of paragpan@gmail.com
Sent: Sunday, February 24, 2013 5:52 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:16859] Pitting Corrosion Resistance Failure in DSS

 

Dear Siva,

Screening refer to the visual examination of the weld joint for any corrosion product like rust, scale present on the external surface.

Each NDE technique has its own limitations in determining the corrosion on the external surface of the weld ment (weld metal,base metal and HAZ).

I can suggest you to pl. go through API RP 571 for your particular type of corrosion and methods to check it.

Regards,

PARAG
Sent from my HTC

----- Reply message -----
From: "Sivaselvam Ponandrum" <sivaselvam@kpoc.com.my>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Subject: [MW:16853] Pitting Corrosion Resistance Failure in DSS
Date: Sun, Feb 24, 2013 1:53 PM

 

Dear Paragpan,

 

What other NDT technique can be used to detect corrosion on the weld?

 

Is there a screening NDT technique (what NDT technique is this?)  prior doing detail NDT?

 

 

Regards

 

Siva

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of paragpan@gmail.com
Sent: Saturday, February 23, 2013 7:03 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:16847] Pitting Corrosion Resistance Failure in DSS

 

Dear Siva,

UT can detect the defects like crack, lack of fusion, LOP etc. in the weldment but not the
Corrosion.

Regards,
PARAG
Sent from my HTC

----- Reply message -----
From: "Sivaselvam Ponandrum" <sivaselvam@kpoc.com.my>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Subject: [MW:16841] Pitting Corrosion Resistance Failure in DSS
Date: Fri, Feb 22, 2013 4:17 PM

 

Dear Team,

 

Can UT Shear Wave detect corrosion at weld joint? Would this be a good screening tool?

 

 

Regards

 

Siva

 

DISCLAIMER: The information contained in this e-mail may be confidential, proprietary, and/or legally privileged. It is intended only for the person or entity to which it is addressed. If you are not the intended recipient, you are not allowed to distribute, copy, review, retransmit, disseminate or use this e-mail or any part of it in any form whatsoever for any purpose. If you have received this e-mail in error, please immediately notify the sender by return e-mail and delete this e-mail and any attachments immediately. Please be aware that the contents of this e-mail may not be secure and should not be seen as forming a legally binding contract unless otherwise stated.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

DISCLAIMER: The information contained in this e-mail may be confidential, proprietary, and/or legally privileged. It is intended only for the person or entity to which it is addressed. If you are not the intended recipient, you are not allowed to distribute, copy, review, retransmit, disseminate or use this e-mail or any part of it in any form whatsoever for any purpose. If you have received this e-mail in error, please immediately notify the sender by return e-mail and delete this e-mail and any attachments immediately. Please be aware that the contents of this e-mail may not be secure and should not be seen as forming a legally binding contract unless otherwise stated.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

DISCLAIMER: The information contained in this e-mail may be confidential, proprietary, and/or legally privileged. It is intended only for the person or entity to which it is addressed. If you are not the intended recipient, you are not allowed to distribute, copy, review, retransmit, disseminate or use this e-mail or any part of it in any form whatsoever for any purpose. If you have received this e-mail in error, please immediately notify the sender by return e-mail and delete this e-mail and any attachments immediately. Please be aware that the contents of this e-mail may not be secure and should not be seen as forming a legally binding contract unless otherwise stated.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

DISCLAIMER: The information contained in this e-mail may be confidential, proprietary, and/or legally privileged. It is intended only for the person or entity to which it is addressed. If you are not the intended recipient, you are not allowed to distribute, copy, review, retransmit, disseminate or use this e-mail or any part of it in any form whatsoever for any purpose. If you have received this e-mail in error, please immediately notify the sender by return e-mail and delete this e-mail and any attachments immediately. Please be aware that the contents of this e-mail may not be secure and should not be seen as forming a legally binding contract unless otherwise stated.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...