Tuesday, February 7, 2012

[MW:13623] RE: 13610] Applicability of Impact testing for Non pressure parts welded on non pressure parts (inside the vessel)

Hi

Impact  test is required for materials such as shell, head, flanges and fittings, stiffener plate or any attachment, if welded to pressure retaining parts, whether internal or external, used for structural integrity, shall be impact tested.

In your case, if SP1 is used in design for structural integrity, then it requires to be impact tested at the same governing MDMT. Please check with your designer. But however, SP2 does not require impact test, since, it is not welded to pressure retaining part. (ref UCS.66)

BR

M.Vijayan

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Aly
Sent: Saturday, February 04, 2012 9:05 AM
To: materials-welding@googlegroups.com
Subject: [MW:13610] Applicability of Impact testing for Non pressure parts welded on non pressure parts (inside the vessel)

 

 

Dear Expert,

 

Kindly advise on following;

 

Suppose I have a vessel with MDMT minus 48deg C, we have support plate (SP1) (inside the vessel) welded with vessels, on which I am going to weld another support plate (Sp2),

 

My question is whether this (SP1 & SP2) required to have impact tested to minus 46deg C or only SP1?

 

Similarly would saddle supports of this vessel require matl with impact testing.

 

Thank you in advance..

 

Ali Mhaskar

UAE

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



This communication and any files transmitted with it are confidential and may also be privileged. It is for the exclusive use of the intended recipient(s). If you are not the intended recipient or the person responsible for delivering it to the intended recipient(s), please note that any form of distribution, copying or use of this communication or information contained in it is strictly prohibited and may be unlawful. If you have received this communication in error please return it to the sender, and delete the material from any computer. We reserve the right to monitor email communications through normal internal and external networks. We believe but not warrant that the email and the attachments are virus free. The statement and opinions expressed in this communication are those of the writer and do not necessarily represent those of Madina Group, whose registered office address is

P.O. Box 20459, Doha, Qatar.
Tel. +974 44600818
Fax. +974 44603143

No comments:

Re: [MW:35289] Welding consumable for S355J2WP material

S355 J2 WP  is a weathering structural steel  It has better atmospheric corrosion resistance. Use E 8018 - W1/W2  Electrodes This is regular...