Hi,
QW-461.9 is for PERFORMANCE QUALIFICATION — POSITION AND DIAMETER LIMITATIONS. i.e,If a welder Qualifies with the position specified in the Qualification test column,will be qualified for the columns specified in the right side.

Now the question raised by Mr.Srinivas is As per ASME Sec.IX,If a WPS qualified with 4G position can be used for 3G welder Qualification or not? For this answer is yes.he can use that WPS for 3G or any position welder qualifications.(with all other essential variables are met)

QW461.9 doesn't restrict for WPS qualification.Change in Position is not an Essential Variable for WPS as Per QW252 to 265.

Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282


--- On Wed, 2/2/11, muthu barathi <muthu_barathi@rediffmail.com> wrote:

From: muthu barathi <muthu_barathi@rediffmail.com>
Subject: Re: Re: [MW:9683] Re: WPS is 4G.. Can i qualify welder in 3G?
To: materials-welding@googlegroups.com
Date: Wednesday, February 2, 2011, 3:55 PM




NO.

Please refer Table 461.9 of ASME sec ix .





On Wed, 02 Feb 2011 14:03:33 +0530 wrote
>ASME Sec.IX - Position is not an Essential Variable for WPS. So 4G WPS
can use for 3G welder qualification with all other EV for welders are
met.(P.No.,F.No., etc.,)

Thanks & Regards,

(Karthik)

Karthikeyan.S QA/QC Manager Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180, Thailand. Phone: 0066 38 897035-8 (Off) Fax: 0066 38
897034 Hand Phone: 0066 892512282

--- On Wed, 2/2/11, muthu barathi wrote:

From: muthu barathi
Subject: Re: [MW:9678] Re: WPS is 4G.. Can i qualify welder in 3G?
To: materials-welding@googlegroups.com
Date: Wednesday, February 2, 2011, 2:58 PM

When
ever you want an answer you have to say complete details then only

you will get the correct answer.



You have to mention what is the code your supporting PQR u can not

change the code of your PQR qualified. according to that u have to

confirm. Ok even as per section IX also you can not qualify the welder.













On Wed, 02 Feb 2011 12:59:06 +0530 wrote

>Dear All.

















If the code is ASME SEC 9.



Can i?







On Feb 2, 12:01 am, Suresh wrote:



> Dear Srinivas ,



>



> I truly agreed with Mr.karthik comment .



>



> Regards



>



> Suresh



>



>



>



>



>



> On Wed, Feb 2, 2011 at 10:23 AM, jaya anil

wrote:



> > Dear Srinivas,



>



> > Welder can be qualified in 3G Position using ur 4G WPS, no issue in

that.



>



> > No need of Qualifying WPS in 3G further .



>



> > Regards



> > Anil



> > On Tue, Feb 1, 2011 at 4:27 PM, Srinivas Engr <



> > srinivas.gmsr...@gmail.com> wrote:



>



> >> Dear all.



>



> >> I have a qualified WPS in 4G.



> >> Can i qualify welders to 3G position as per 4G wps without WPS



> >> qualification?



> >> Pl advise me. Its urgent.



>



> >> Thanks



> >> Srinivas



>



> >> --



> >> To post to this group, send email to materials-

welding@googlegroups.com



> >> To unsubscribe from this group, send email to



> >> materials-welding+unsubscribe@googlegroups.com

welding%2Bunsubscr­ibe@googlegroups.com>



> >> For more options, visit this group's bolg at



> >>http://materials-welding.blogspot.com/



> >> The views expressed/exchnaged in this group are members personel

views and



> >> meant for educational purposes only, Users must take their own

decisions



> >> w.r.t. applicable code/standard/contract documents.



>



> > --



> > To post to this group, send email to materials-

welding@googlegroups.com



> > To unsubscribe from this group, send email to



> > materials-welding+unsubscribe@googlegroups.com

welding%2Bunsubscr­ibe@googlegroups.com>



> > For more options, visit this group's bolg at



> >http://materials-welding.blogspot.com/



> > The views expressed/exchnaged in this group are members personel

views and



> > meant for educational purposes only, Users must take their own

decisions



> > w.r.t. applicable code/standard/contract documents.



>



> --



> Thanks & Best Regards,



>



> Suresh



>



> Mobile No: 91-92 92 905 905- Hide quoted text -



>



> - Show quoted text -







--



To post to this group, send email to materials-welding@googlegroups.com



To unsubscribe from this group, send email to materials-

welding+unsubscribe@googlegroups.com



For more options, visit this group's bolg at http://materials-

welding.blogspot.com/



The views expressed/exchnaged in this group are members personel views

and meant for educational purposes only, Users must take their own

decisions w.r.t. applicable code/standard/contract documents.





Dear Sir,











Thanking You,



Honesty is the best Policy



With Warm Regards,



Muthu Barathi P

Mobile No:00962788269821 (Jordan)

00962775401951




--

To post to this group, send email to materials-welding@googlegroups.com

To unsubscribe from this group, send email to materials-
welding+unsubscribe@googlegroups.com

For more options, visit this group's bolg at http://materials-
welding.blogspot.com/

The views expressed/exchnaged in this group are members personel views
and meant for educational purposes only, Users must take their own
decisions w.r.t. applicable code/standard/contract documents.








--
>
To post to this group, send email to materials-welding@googlegroups.com
>
To unsubscribe from this group, send email to materials-
welding+unsubscribe@googlegroups.com
>
For more options, visit this group's bolg at http://materials-
welding.blogspot.com/
>
The views expressed/exchnaged in this group are members personel views
and meant for educational purposes only, Users must take their own
decisions w.r.t. applicable code/standard/contract documents.
>


Dear Sir,





Thanking You,

Honesty is the best Policy

With Warm Regards,

Muthu Barathi P
Mobile No:00962788269821 (Jordan)
00962775401951

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...