Tuesday, February 15, 2011

Re: [MW:9881] Groove design and bevel

Dear Bharat,

If I were you, i would have followed the groove design shown in ASME B31.3 and also in your case Contractor was also not agreed which means at later stage, Contractor would raise this issue if something goes wrong. 

but again, other groove design are also available and has been used successfully,

Regards
Manpreet Singh



On Mon, 14 Feb 2011 17:16:19 +0530 BHARAT GOLE <bharatgole@hotmail.com> wrote
> Dear Manpreet,
>I would like to share my experience realted to same issue which is raised by Mr. Husain.
>In our previous project we received fittings thickness greater than 22 mm with compound bevel .However pipes received with single bevel.Then contractor propose to do compound bevel for pipes with additional work and of course with extra cost.
>Construction code ASME 31.3 & approved WPS was without Impact, with PWHT as per ASME IX .
>WPS/PQR was qualified by Ludwing (one of reputed TPI ) showing various combination of joint configurations.Based on that we told contractor to go ahead with welding as it is - i.e.one side compound bevel & other side single bevel
>So there was big noise between contractor & us....contractor was not ready to weld joint like that
>Please let me know then my interpretation was correct or not ?
>Warm regards
>
>Bharat

>

>

>
>
>
>
Date: Mon, 14 Feb 2011 06:28:05 +0000
>To: materials-welding@googlegroups.com
>Subject: Re: [MW:9866] Groove design and bevel
>From: manpreetsin88@rediffmail.com
>
>Dear Husain,
>
>I guess your design code is ASME B31.3, ASME Sec ix do not go into process details (bevel preparation etc.)
>
>With reference to the butt end preperation shown in Fig 328.4.2 , Manufacturer has provided pipes withcompound bevel as required by code, now you need to confirm whether bevel preperation done at site is in accordance with Fig 328.4.2.
>
>Regards
>Manpreet Singh
>
>

>
>On Sun, 13 Feb 2011 21:42:00 , Ahmed Husain <ahmraha@yahoo.com> wrote
>

Dear All,

I have a query, kindly share your valuable knowledge on this subject.

1-As per ASME IX, Table QW-253 and QW-256, groove design is non-essential variable for SMAW and GTAW welding.

2-As per ASME B31.3, Fig 328.4.2 and ASME B16.25 Fig 3 and 5 (also Para 3.1C), components having thickness above 22 mm shall have compound bevel.

I would like to know that if the requirements of ASME B31.3 and 16.25 as stated above are mandatory? Because as per SEC IX, it is non-essential variable.

What I have observed at site, all pipes and fitting above 22 mm thickness have compound bevel from manufacturer, but all bevel prepared at side are single bevel. Is this acceptable?


>
Ahmed Husain
>Mob-0547170325

>
>--
>To post to this group, send email to materials-welding@googlegroups.com
>To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>
>
>--
>To post to this group, send email to materials-welding@googlegroups.com
>To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>

--
>To post to this group, send email to materials-welding@googlegroups.com
>To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...