Re: [MW:9027] Re: Stress Corrosion Cracking Test


Dear Mr. Herman

Thanks for quick reply.

It is not mistake in specification. Specification categorically demands 40% CaCl2 solution (Ph -6.5, Testing time - 500 Hrs., 100 Deg Boiling, Acceptance criteria - Stress to cause rupture shall exceed 0.85 times UTS, as per ASTM G 46)

Further, specification calls for  MgCl2 solution for Duplex grade as per G 36.

Since, aberrant solution is being asked for testing as per ASTM G 36, precisely the question was put in this forum.

Request all team members to share views of chloride stress corrosion test of super Duplex ( S 32750)

With Best Regards,

Jignesh R Rana
Manager - QA & QC

Linde Engineering India Pvt. Ltd.
38, Nutan Bharat Society, Alkapuri, Vadodara 390007, India
Tel.: +91 265 3056789, Fax: +91 265 2335213 , Mobil:  +91 90999 86019
jignesh.rana@linde-le.com, www.linde-india.com

This e-mail is confidential. If you are not the intended recipient, please notify us immediately. You should not disclose its contents to any other person nor use it for any purposes.





hpi001 <pieper-qsi@kpnmail.nl>
Sent by: materials-welding@googlegroups.com

30/12/10 16:53

Please respond to
materials-welding@googlegroups.com

To
"Materials & Welding" <materials-welding@googlegroups.com>
cc
Subject
[MW:9019] Re: Stress Corrosion Cracking Test





Why does anyone asking for ASTM G36 with an aberrant test solution?
Probably there will be no big difference between both solutions
because Chloride is the important part in this test but by choosing
for CaCl you won't have any reference or acceptance criteria or is
this also specified in the project specification? Can it be a mistake
in the specification as well?

Best Regards,

Herman Pieper

On 30 dec, 11:44, jignesh.r...@Linde-LE.com wrote:
> Dear Members,
>
> One of our project specification calls for Chloride Stress Corrosion
> Cracking as the ASTM G 36 with CaCl2 (40%) solution for super Duplex
> Stainless steel ( S 32750)
>
> ASTM G- 36 is based on MgCl2 solution.
>
> Does any one having experience with SCCT with CaCl2 solution ?
>
> With Best Regards,
>
> Jignesh R Rana
> Manager - QA & QC
>
> Linde Engineering India Pvt. Ltd.
> 38, Nutan Bharat Society, Alkapuri, Vadodara 390007, India
> Tel.: +91 265 3056789, Fax: +91 265 2335213 , Mobil:  +91 90999 86019
> jignesh.r...@linde-le.com,www.linde-india.com
>
> This e-mail is confidential. If you are not the intended recipient, please
> notify us immediately. You should not disclose its contents to any other
> person nor use it for any purposes.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...