Mr. Mehta,
From the description this material is a cast martensitic stainless steel.The close and popular ASTM/ASME grade would be A/SA743/CA6 NM.
GX$CrNi13-4 + QT, stands for cast martensitic stainless steel. I think you're missing one digit (see the number marked in red) in your description, that indicates Carbon percentage.See the attached sulzer document for your reference.
What's the intended use of this material? Hydro turbine blades or any Oil and gas applications??
Welding of this steel is possible as follows:-
- Matching chemistry-E/ER-410NiMo
- Dissimilar Chemistry--Austenitic S.S E-ER-309L
- Dissimilar Chemistry- Nickel Based Electrodes-Inconel-ENiCrFe3
Let's know the design parameters for the best welding recommendations.
Thanks.
Pradip Goswami,P.Eng.IWE
Welding & Metallurgical Specialist & Consultant
Email-pgoswami@sympatico.ca,
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of B D Mehta
Sent: Wednesday, December 29, 2010 5:45 PM
To: materials-welding@googlegroups.com
Subject: [MW:8977] welding repair of material GX$CrNi13-4 + QT
Dear all
Any body cal tell me about the selection of electrode for doing welding repair of material GX$CrNi13-4 + QT
Thanks and regards
B.D. Mehta
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.