Skip to main content

[MW:1992] Re: cleaning of copper pipes

Speciality Chemicals are available from reputed Manufacturers and can be referred to

B. Rgds.

G. A. Soman
Don Bosco Maritime Academy

----- Original Message -----
From: "Bathula Raghuram (Mumbai - PIPING)" <R.Bathula@ticb.com>
Date: Monday, April 20, 2009 9:11 am
Subject: [MW:1991] RE: cleaning of copper pipes
To: materials-welding@googlegroups.com

> No idea about pipes. But the standard method for cleaning copper wire
> rod during wire drawing process is pickling in hot 20% sulfuric acid
> followed by rinsing in water.
>
> Any suggestions from members?
>
> ________________________________
>
> From: venu moturu [mailto:moturuvenu@yahoo.com]
> Sent: Sunday, April 19, 2009 5:30 AM
> To: Bathula Raghuram (Mumbai - PIPING); sanjay
> Subject: cleaning of copper pipes
>
>
>
> Dear Raghu,
>
>
>
> Could you pl. advice/ suggest me any procedure / cleaning method
> available for removing tarnish on copper pipes ....
>
>
>
>
>
> Regards
>
> venu
>
>
>
>
> >
>

DON BOSCO MARITIME ACADEMY
Premier Automobiles Road,
Kurla West, Mumbai 400070
Tel: (022) 2504 1585 / 2018; 25036344. Fax: (022) 2504 0682
Email: donboscomarine@vsnl.net
Website: www.dbma.in

--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Re: [MW:14950] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

Dear All, I have been a CONSULTANT FOR such problem & my personal opinion is expressed as follow. I fully agree with views expressed so far. But bag to differ that " Code is a law, with engineering judgments. Hence the inspector has the rights to declare that the original HT was inadequate." Inspectors & total industry must resist the "REJECTION" . We as intellectual & having seniority must become practical. How the code will revise???. ANS.: One is experiments (Pure research) & second is such chances that gives opportunity to experiment !!! _______________________________________________________________________________________________ My understanding is that it is P1 material. In that case every pass normalizes the immediate bottom pass. Hence code requirement for P1 FOR MANDATORY SR is 32 mm & above thickness. SOLUTION:  In any case 0. After SR=PWHT no PTC testing is required as per code--Unless for low temp. vessels. That means code ...