Re: [MW:30682] Welding and cladding SA-516 Gr. 60 + AISI 410S

Please see API 582

On Wed, Apr 1, 2020, 7:56 PM Caro <carolinamreinoso@gmail.com> wrote:
Hello, 

I have the same case, A516gr60 +410S, Which filler metal is recommended for FCAW process? 

thanks in advance,


On Tuesday, May 28, 2013 at 3:42:46 AM UTC-3, Ramin Kondori wrote:
Dear Branko:

Depositing AISI 410S on A516 will produce a martensitic weld overlay which is prone to cracking even during welding. There Are two solutions:
  1. Using a buffer layer (intermediate layer) of E309L or even E310L on A516 and then Depositing 410S
  2. Applying preheat of min 250-300 C which makes it a very hard job though it may seem less expensive

In first scenario, you do not need any preheat but I do not recommend using SAW for 410S layer since it may melt through the buffer layer and reach A516 which maybe, maybe causes problems. You can use GMAW with Ar+2%o2 or Ar+3%CO2. Do not forget the Preheat...

This way your weld overlay will be thicker than 3 mm and you should weld a PQR coupon to make sure you have 3mm of 410 weld layer "over" the buffer layer. Maybe you'll have to deposit one buffer (309L or 310L) and 2 layers of 410S. Try using Pulsed GMAW to get the results with depositing one layer.

One of our colleagues have successfully deposited one layer of 410 weld overlay on A516 using Pulsed-MIG (Preheat is essential). It's because Pulsed-MIG has less dilution and you may achieve required results in one layer.

For PQR, you need 4 side bend tests, chemical analysis on the surface of overlay and 3-4mm below the surface, and hardness test (on the surface).

Discuss these issues with your client before proceeding.

Good Luck
Ramin Kondori
Sr. QA/QC Engineer
SINOPEC

r.ko...@petroyada.com
+98-2123592322
+98-9132150320



On Mon, May 27, 2013 at 4:37 PM, Branko Ferencak <bran...@gmail.com> wrote:
I have shell 20mm thick ( SA-516 Gr, 60 ) and there must be cladd AISI 410S 3mm    
Could anybody tell me which filler i can use, for SAW  and GMAW?
GMAW i  planning use for flanges and tubesheets ( after i overlay tubesheet - what is procedure for welding tube to tubesheet? )
Also PWHT has been asked by customer after overlay. 
Can anybody tell the effect of PWHT on SS 410S overlay? 
What will be the the safe range of temperature of PWHT?  ( Also recommended temperatures and times, holding cooling...)

Best regards,
Branko Ferencak

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to material...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/4c78b169-002a-4e15-9796-4dad639c3ef1%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJBR2%2BPRCRVkVXm%3D-sDEYKb%2Bc4W7cOWhPv6%3DhHUCquGph9m7YA%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...