Skip to main content

Re: Re: [MW:29165] RE: 28982] Backing gas as per API RP 582

Dear All:

Below you can find a screen shot from SLV Duisburg publication:
"Guidelines on the Welded Fabrication of Stainless Steels"

SLV publications are among the most reliable references in welding engineering 
and here, it clearly states that in single side welding of SS, the other side must either be protected or the oxide layer be removed.



Regards
Ramin  Kondori
Sr. QA/QC & Welding Engineer
-----------------------------------------------------------
PG-Dip. in Welding Engineering (IWE  AT  0070)
BSc. in Civil Engineering (IUT)
BGAS Painting Inspector
ASNT Level I&II
                        
IIW-Logo-Colour-small


On Wed, Feb 27, 2019 at 4:12 PM muneebslsa@gmail.com <muneebslsa@gmail.com> wrote:
You can check the attchments, but anyhow when it comes to thinner membrane regardless of whatever the consequences might be the case for oxidation which is non occurrence when we simply imagine for fillet welds but anyhow socket welds aren't with this case of lap to lap fillets, hence a detailed study of amendment to be incorporate with through and through case studies and failure analysis stipulating clauses shall be ensured in international standards.

Anyhow now the case as per the research is chromium depletion (causing heat tints / discoloration) for thinner membranes especially for fillets, So to be conclude that there should be some detailed studies as per AWS D18.2 / NORSOK STANDARD M-601 especially for fillet welds.

At any cost don't accept the requirement unless owner is providing his clause which is already stipulated in owner's manual or international standards, the research i have ensured is from my previous owner requriement which i did not agree and the international standards which i have quoted is for open root / butt welds.

Thanks.


Regards,
MOHAMED MUNEEB MAHABOOB

 
Date: 2019-02-24 11:20
Subject: Re: [MW:29146] RE: 28982] Backing gas as per API RP 582
To be specific, as you know purging purpose in SS is mainly for shield against oxidation which took place when molten metal kiss the oxygen from atmosphere. Now when you welding a fillet weld the amount of oxidation is corresponding to the amount of heat supplied vs. encounter of molten weld metal to the atmosphere without shielding. 

A fillet weld having a configuration without any gap and zero flow of molten metal to the back side will defiantly not require any purging. Its recommended to use a optimized low heat input. I advise you although to put gas backing upto 2 mm thickness as the low heat dissipation in SS can melt through thickness during welding.

Thanks & regards
Sandeep Kumar

On Friday, February 22, 2019 at 6:19:06 AM UTC+3, John Manoj wrote:
Thanks for the reply, Is back purging is required when we do fillet welding on a thin (2mm to 5mm) SS base material, for example some cleat welding or pad welding or socket welding with GTAW or SMAW process.

Expecting a reply.
Thanks,
Manoj

Dear Mr. Goswami,

In 2016 editions of API RP 582 the purging gas requirement given in subcluases (a) (b) (c) but in previous editions purging requirement given in clause 

On Mon, Jan 28, 2019 at 9:53 AM PGoswami <pgos...@quickclic.net> wrote:

Manoj,

 

SMAW never requires back purging. It's the "slag" generated by the process, which protects the weld root. This is just back to basic scenario.

Thanks.

 

P.Goswami.P.Eng, IWE.

Independent Welding & Metallurgical Specialist

Saudi Aramco: Designated Project Welding Engineer(DPWR)& Quality Management Personnel

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:p...@quickclic.net,pradip.goswami@gmail.com

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of Manoj John
Sent: January 27, 2019 8:04 PM
To: material...@googlegroups.com
Subject: [MW:28982] Backing gas as per API RP 582

 

Dear Experts,

 

As per clause 7.3 of API RP 582 Ed. 2016 back purging required for GTAW & GMAW process but no where I could found for other process like SMAW.  Is it mean that if we do welding with SMAW process back purging is not required?

 

Please share your interpretation.

 

Thanks and regards

 

Manoj.

 

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Re: [MW:14950] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

Dear All, I have been a CONSULTANT FOR such problem & my personal opinion is expressed as follow. I fully agree with views expressed so far. But bag to differ that " Code is a law, with engineering judgments. Hence the inspector has the rights to declare that the original HT was inadequate." Inspectors & total industry must resist the "REJECTION" . We as intellectual & having seniority must become practical. How the code will revise???. ANS.: One is experiments (Pure research) & second is such chances that gives opportunity to experiment !!! _______________________________________________________________________________________________ My understanding is that it is P1 material. In that case every pass normalizes the immediate bottom pass. Hence code requirement for P1 FOR MANDATORY SR is 32 mm & above thickness. SOLUTION:  In any case 0. After SR=PWHT no PTC testing is required as per code--Unless for low temp. vessels. That means code ...