No purging require while doing SMAW welding for most of materials with few exceptions. 
While welding root with SMAW, the process generate enough gases around the weld puddle which is sufficient to protect it from both sides & remember gases have passes to go backside from one side of unwelded area as well as though the molten pools which have high solubility for gas and very fast release during solidification due to high cooling rate.


Thanks & regards
Sandeep Kumar

On Thursday, February 21, 2019 at 10:04:44 AM UTC+3, Bathula Anil Kumar wrote:
I Feel Even in Root , if Welding is done with SMAW, Back purging is required, in Covered electrodes slag is formed in the outer surface , it will not protect inside, Since SS is highly volatile and readily absorb atmosphoric gases, back purging is required

Thanks & Regards,

Bathula Anil Kumar

PH N0: +91-7675019922



On Tue, Jan 29, 2019 at 3:27 PM George Dilintas <dili...@gmail.com> wrote:
Slag is lighter than molten steel. It will come up to the surface. I wonder thait will protect the root. Usually we do 5mm with purging and gas backing using GTAW and then we switch to SMAW 

Στις Δευ, 28 Ιαν 2019, 07:53 ο χρήστης PGoswami <pgos...@quickclic.net> έγραψε:

Manoj,

 

SMAW never requires back purging. It's the "slag" generated by the process, which protects the weld root. This is just back to basic scenario.

Thanks.

 

P.Goswami.P.Eng, IWE.

Independent Welding & Metallurgical Specialist

Saudi Aramco: Designated Project Welding Engineer(DPWR)& Quality Management Personnel

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:p...@quickclic.net,pradip.goswami@gmail.com

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of Manoj John
Sent: January 27, 2019 8:04 PM
To: material...@googlegroups.com
Subject: [MW:28982] Backing gas as per API RP 582

 

Dear Experts,

 

As per clause 7.3 of API RP 582 Ed. 2016 back purging required for GTAW & GMAW process but no where I could found for other process like SMAW.  Is it mean that if we do welding with SMAW process back purging is not required?

 

Please share your interpretation.

 

Thanks and regards

 

Manoj.

 

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...