ASTM NO                                                     No Of Grains/square mm  at  100X                                         Remarks
 1                                                                                   upto 1-1/2
2                                                                                    1 1/2-3 
3                                                                                      3-6
4                                                                                      6-12
5                                                                                      12-24
The above are having coarse grain which is best for creep resistance because of less grain boundary  

6.                                                                                    24-48
7                                                                                     48-96
8                                                                                     96 and over
The above are having fine grain Which is best for mechanical properties because more grain more strength 

hope that it is clear now.
  


THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


On Wed, Feb 13, 2019 at 7:45 AM ishwar kumar <ish8623@gmail.com> wrote:
1,2,3,4,5 Coarse grain and 6,7,8 fine grain

On 12-Feb-2019, at 6:18 PM, sandeep kumar <sandeepdhiman63@gmail.com> wrote:

Hi Ramin

Please note, my question is what does mean the coarse?
a higher ASTM no or smaller no.

Thanks.

On Monday, February 11, 2019 at 5:24:06 AM UTC+3, Ramin Kondori wrote:
This number is related to the Number of grains in an specific area.
higher number of grains means they are smaller grains or fine grain.


Ramin  Kondori
Sr. QA/QC & Welding Engineer
-----------------------------------------------------------
PG-Dip. in Welding Engineering (IWE  AT  0070)
BSc. in Civil Engineering (IUT)
BGAS Painting Inspector
ASNT Level I&II
                        
IIW-Logo-Colour-small


On Sun, Feb 10, 2019 at 2:22 PM sandeep kumar <sandeep...@gmail.com> wrote:
Dear all

Please advise your views on below query:

ASTM A182 10.1.2 Grades F 321H, F 347H, and F 348H shall have a
grain size of ASTM No. 7 or coarser.


What does it stand for coarser? 
Does it mean a higher ASTM grain size no (e.g. 8, 9 and so on) or lower ASTM grain size no. (e.g. 6, 5, 4 and so on)?


Thanks & regards
Sandeep 

-- 
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
--- 
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

-- 
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
--- 
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...