I fully agree Jurgen Prinsen.
-- I think on our material specification, we should clearly indicate that the hardness should not be higher than 200 brinell.
On Tuesday, February 12, 2019 at 9:16:02 AM UTC+7, Jurgen Prinsen wrote:
On Tuesday, February 12, 2019 at 9:16:02 AM UTC+7, Jurgen Prinsen wrote:
This 200HB is only mentioned as in delivery condition, not in as welded condition.As welded hardness depends on chemistry and cooling rate (e.g preheat, heat-input, wall thickness)RegardsJurgen Prinsen IWE/MScWeld-Tech BVWelding consultancy and engineering since 1988Van: "JosƩ Juan JimƩnez Alejandro" <jjjim...@gmail.com>
Aan: material...@googlegroups.com
Verzonden: Zondag 10 februari 2019 18:09:34
Onderwerp: Re: [MW:29081] Hardness for SA516 Grade 70I was looking for that data in the Code, I could not find it, hopefully someone has better luck and share the hardness data of this steel, with reference to the standard; On the other hand, when a pressure vessel carries the ASME stamp, the Authorized Inspector of the Authorized Inspection Agency necessarily has to intervene with your company has a contract, the Authorized Inspector has the obligation to advise and give you technical support.El dom., 10 feb. 2019 a las 6:42, BCK 055 (<bck...@gmail.com>) escribió:PWHT is followed spec, and WPS should be shown hardness test value.Sent from my Blackberry
From: RKDSent: Sunday, February 10, 2019 17:52To: Materials & WeldingReply To: material...@googlegroups.com Subject: [MW:29073] Hardness for SA516 Grade 70For a pressure vessel designed with stamped under ASME VIII Div.1, there is a requirement that: "Hardness values should not exceed 200 brinell for the welds / material of shell."
Shell material is specified as SA516 Grade 70.
I am concerned the requirements for hardness and material will automatically require stress relief for all pressure vessel parts.
Would SA516 Grade 70 have hardness lower than 200 Brinell?
Thank you.
Regards,
RKD
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com .
Visit this group at https://groups.google.com/group/materials-welding .
For more options, visit https://groups.google.com/d/optout .
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com .
Visit this group at https://groups.google.com/group/materials-welding .
For more options, visit https://groups.google.com/d/optout .--Ing. JosƩ Juan JimƩnez Alejandro
ASME Independent Consultant
and Technical Manager SSI-TPI
Cel. +52 812 352 4606
Skype: jjjimeneza
Twitter: @jjjimeneza
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com .
Visit this group at https://groups.google.com/group/materials-welding .
For more options, visit https://groups.google.com/d/optout .
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Comments