Re: [MW:28356] Reg:SS to MS support welding

You can use MS cleats buttered with E 309 electrode for minimum of 3
layers. This helps to avoid contamination and carbon pick up on SS plate.
On MS plate, there will not be any issue.
C Sridhar
-----------------------------------------

On Friday, 28 September, 2018, 9:54:48 AM IST, George Dilintas <dilintas@gmail.com> wrote:


Boxbe This message is eligible for Automatic Cleanup! (dilintas@gmail.com) Add cleanup rule | More info
The contamination will not affect the test piece. However in production contamination has to be avoided

Στις Πέμ, 27 Σεπ 2018, 13:55 ο χρήστης Gopalakrishnan G <gopal2408@gmail.com> έγραψε:
Dear experts
I want to do PQR for ss304L to is2062.my doubt is what material to be used for support to avoid distortion ? whether SS or MS ?.if I use MS for support any contamination will reflect in test piece?.kindly guide me.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

I'm protected online with Avast Free Antivirus. Get it here — it's free forever.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...