Skip to main content

Re: [MW:26268] Shielding gas for GMAW pulsed welding-Carbon Steel

Dear Pandithan,

Here the wire I am using is of dia 1.2 mm. So is it possible to give the current & voltage of that range in the weld layers? The welding process I am following is Root & hotpass TIG and the balance MIG. 

Regards,
Aby

On Wed, Mar 22, 2017 at 3:36 PM, Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:
Voltage anything less than 21v goes to short circuit, but in ur case Voltage is ok, but increase the current to minimum 250amps, Do not put in Synergy mode and set the Current as required.

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Wed, Mar 22, 2017 at 10:06 AM, Aby Jose <abycscec@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (abycscec@gmail.com) Add cleanup rule | More info

Dear Mr Pandithan,

In the machine I have selected the pulse mode itself. (GMAW-P). The position I am using is IG(rotating ) . As I am using the synergy mode in the machine the current and voltage is getting selected automatically when I am giving the wire feed speed. I am using the wire feed speed of 9.5 m/min, the voltage coming is in range 25V -28V and current in range 215 to 230. How to ensure I am not using the short circuiting mode?? I am using this process for pipe welding which includes both high and low thickness.

Regards,
Aby

On Wed, Mar 22, 2017 at 9:02 AM, Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:
As argon increase, %of penetration will come down and may get into porosity .  Try with 85+15 with current of >250amps. spatter is inevitable in this process, u can reduce by another option with GMAW-P. If u work in Spray mode, spatter stiking into base metal will be less due to its sizes

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Tue, Mar 21, 2017 at 7:12 PM, Prasad Rao <prasadrao31@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (prasadrao31@gmail.com) Add cleanup rule | More info

Try for 98% argon and 2% co2

On Tue, Mar 21, 2017 at 12:56 PM, Aby Jose <abycscec@gmail.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (abycscec@gmail.com) Add cleanup rule | More info

Dear all,

What shielding gas should be used for the pulsed GMAW welding of carbon steel? When trying with 80%Ar+20%CO2 mixture I am getting a lot of spatters. The welding used is Automatic welding with Robotic machine.
Any recommendations???

Regards,
Aby

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACdTRdyc8NMn6LBHHHTeYFxP_Ani0cnWDw0j5qEJSyRyfoOe4Q%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAEML-XRowcwexs%3DZz4xzozQA7Q6p6XcbJr1YNpG98vBsr-o90w%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eMRjCwxaG%3DH62vgm57nrFmJuf8rLFrZX%2BW9Tah%3D0wjHJg%40mail.gmail.com.

For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACdTRdzxfYOOSzPmY0MZP09YPVeAXwyREZSr9%2B6GyYUGdL0%2BTg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eNWOeQx1Wd5ya-5bGNh1EdvH5tNu8T%3D%3DEY%2Bbs1CQU3p3A%40mail.gmail.com.

For more options, visit https://groups.google.com/d/optout.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACdTRdz2P9cghC0P9%2BbD_SNzioyvo_XugpZFB0RBbQUJDajz%3Dg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .