Skip to main content

Re: [MW:23921] Bulge P-91 Pipe after PWHT

Pls find attached typical arrangement. Pipe is 10" with 12.7mm thickness

On Tue, Nov 24, 2015 at 8:28 PM, Thompson, Dennis <Dennis.Thompson@teaminc.com> wrote:

Hi Pradip,

 

Thanks for emailing us the temperature-time chart.

 

However, we still need a sketch or drawing of the heater and thermocouple arrangement.

 

You stated that you utilized 2 thermocouples, 180o apart.  However, where were they relative to their heaters and relative to the header-tube weld?

 

Specifically:

 

1.      What are the diameters and thicknesses of the header and tube(s)?

2.      What size heaters were attached to the header, and where were they and their control thermocouples relative to the location of the header-tube weld?

3.      What size heater was attached to the tube, and where was it and its thermocouple relative to the header-tube weld?

4.      The fact that the softened, bulged section of tube was 140 mm from the header-tube weld indicates that the temperature of the tube at that location may have exceeded the PWHT soak temperature.

5.      Your sketch/drawing of heater sizes and thermocouple locations will help diagnose the cause of your problem.

 

Regards,

Dennis

 

 

 

From: pradip kumar Sil [mailto:pradipsil@gmail.com]
Sent: Tuesday, November 24, 2015 6:45 AM
To: Thompson, Dennis; materials-welding


Subject: Re: [MW:23914] Bulge P-91 Pipe after PWHT

 

Dear Dennis,

Pls find the PWHT chart & in 10" we used two nos of thermocouple with equal distance i.e 180 degree. We checked the hardness in the weldment as well as HAZ zone & found 210 to 238 HB but in bulge zone ( Parent Material ) which is 140 mm away from weldment is coming 155 to 175 HB.

Thanks in advance.

Regards,

Pradip

 

On Tue, Nov 24, 2015 at 4:22 PM, Thompson, Dennis <Dennis.Thompson@teaminc.com> wrote:

Hi Pradap,

 

Please email us a drawing of the heater and thermocouple arrangement that was employed for your PWHT, along with a copy of your temperature-time chart.  Both are needed to help diagnose your failure.

 

Regards,

Dennis Thompson, P. E.

Team IHT Technical Support Manager

973-885-2148

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of pradip kumar Sil
Sent: Tuesday, November 24, 2015 5:37 AM
To: materials-welding
Subject: Re: [MW:23914] Bulge P-91 Pipe after PWHT

 

It is not possible to do PWHT horizontally because spool piece is welded at location

 

On Tue, Nov 24, 2015 at 3:25 PM, VHEER RAJHU <rajuveera2011@gmail.com> wrote:

Mr shanmugan,

Job is kept in vertical condition where and when the job is heated locally the material softens  at that particular area where all the weight of the job is acted on that softened area which leads to bulging locally

Preferred to do PWHT HORIZONTALLY

On 24 Nov 2015 14:46, "shanmuganathan .subbiah" <shanmuganathan.subbiah@gmail.com> wrote:

Dear 

 

Both end closed or not during PWHT?

 

 

On Tue, Nov 24, 2015 at 12:26 PM, pradip kumar Sil <pradipsil@gmail.com> wrote:

Dear Expert,

In P91 Material ( HRSG header Joint ) after pwht one joint is bulge.We did  Preheating ,Welding , Post Heating,& PWHT in proper way.

Can anybody explain why this bulge occurs & remedy.

During fit-up inspection & weld visual inspection all round the joint is perfect but after PWHT pipe is bulge 140 mm away from the   weld ment

Pic Attached

Regards,

Pradip

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAB%3DAs8kfusRiywON4c0YxkK74WcPtsqTEFnp9QH-4KyzX%2BrSrA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.



 

--

Regards

SHANMUGANATHAN SUBBIAH

AIB- Vincotte International & Partners LLC

PO.Box-420, PC -116

MAF, Sultanate of Oman

Tel: +968 24565771

Fax: +968 24565772

Mob: +968 92096714

Web:www.vincotte.com

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAD2bsBTodkTQm%3DdqiJ2XZ70MFxExzinYdhn4fHJ96StPy1A6WQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.

To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFz2VvSzYO2qNL6SWL4ww0jhoRZLxcr2GRp%2Bc9%3DfN9uuKiAUBg%40mail.gmail.com.


For more options, visit https://groups.google.com/d/optout.

 

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.

To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAB%3DAs8nALCfhN%3DG6V5%3DA%2BHnJYRw85%3DGXNoUFSCQfxYiQvrqtYw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

 


--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAB%3DAs8mkUHsRXDvHW--VH%3DrtAm3Hx4B%2Bp7dKaos%3DUg0qQDh9nQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...