Re: [MW:23862] WQT minimum requirement while using 2'' test coupen

hi,
Minimum - 150mm.
Q W - 3 0 2 . 2 V o l u m e t r i c N D E . When the welder or
welding operator is qualified by volumetric NDE, as permitted in QW-304 for welders and QW-305 for welding
operators, the minimum length of coupon(s) to be examined shall be 6 in. (150 mm) and shall include the entire
weld circumference for pipe(s), except that for small diameter pipe, multiple coupons of the same diameter pipe
may be required, but the number need not exceed four
consecutively made test coupons. The examination technique and acceptance criteria shall be in accordance with
QW-191.


 
Thanks& Regards,
 
(Karthik)
QA/QC Manager 
CMI-Thai Services Co.,Ltd. 
50/35 Sermsuwan Road,Tambol Maptaphut 
Amphur Muang Rayong,Rayong 21150
Thailand
www.cmi-services.com 
Tel : +66 38 691 390-2 ext.103 
Fax : +66 38 682 338 
Mobile: +66 892512282 
E-mail : karthikeyan@cmi-services.com
               Karthik6684@yahoo.com



On Saturday, November 7, 2015 11:25 AM, MANIK <manik.tr2000@gmail.com> wrote:


Dear all

What is the requirements while using 2'' test coupon for WQT?
As i need to prepare 2 numbers of 2" test coupon for one welder.
I assume, it will be minimum circumferential length to be welded, if so how much?
Where shall i find the note in sec IX?

Manik
Piping Supervisor. 
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/202ec153-896e-4bb3-a56c-f998e04eb6f3%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...