Usually during welding, you use earthing connection. Try to add 2 more earthing connections and weld, sure it will demagnetised during welding.
Usually we follow the same for welding of 9%Ni steeel
Sent from my iPhone
Sent from my iPhone
--We have preheated up 250 deg C but no result...please suggest the Preheat Temp.From: Manoj SinghSent: Tuesday, April 07, 2015 7:25 PMSubject: Re: [MW:23051] Magnetization of A 335 P11/P12 during grinding process [GroupMail]Do preheat before welding do demagnetize it--On Tue, Apr 7, 2015 at 2:54 PM, Don Under Survilliance <donsaab3@gmail.com> wrote:
wrap the copper coils around the job at location and ground it. it will surely helpTo view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAM6T1-EfX8LRSJaUtwXSOD4ad7Y0764eXLW00OwpRRofD8qQ7w%40mail.gmail.com.--On Tue, Apr 7, 2015 at 12:36 PM, B Osare <bosare@nfl.co.in> wrote:
--Dear Experts,We have observed that piping material A 335 P11 & P12 of Super heater Header Tee size 12"& 18" (Thickness 45.00 mm & 65.00 mm respectively) was magnetized during grinding process at Location (not in workshop). Can anyone tell us how this phenomenon occurs and how it can be de-magnetize at job location? The weld material is getting cracked after welding. Please suggest the welding procedure with suitable welding electrodes & what precautions to be taken during welding.RegardsB OsareFrom National Fertilizers Limited, Vijaipur
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CE2FEBA545354C0C93B2B0585FD87FE4%40mechworkshop.
For more options, visit https://groups.google.com/d/optout.
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPkJdRLdY9rMveU9_zzDKXmBT9PPKbMusoBs1S170R4Fo9SpXA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/409DCE51B8F44B88BCC061077E473A4F%40mechworkshop.
For more options, visit https://groups.google.com/d/optout.
No comments:
Post a Comment