Skip to main content

RE: [MW:22701] tube to tubesheet welding

Hello Venkatesh,
 
Tube to tube sheet welding is a special kind of welding, both process and technique wise.. Essentially the parameters , techniques adopted for a groove weld will not work for this type of weld joint.
 
A separate procedure and performance qualification is required.
 
Please see some of the extracts from Sec-IX,QW-193 below.
 
Hope this will clarify your query.
 
Thanks
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 

QW-193 TUBE‐TO‐TUBE SHEET TESTS

When the applicable Code Section requires the use of this paragraph for tube‐to‐tube sheet demonstration mockup qualification, QW-193.1 through QW-193.1.3 shall apply.

QW-193.1 Procedure Qualification Specimens. Ten mockup welds are required to qualify each procedure. The mockup assembly shall essentially duplicate the tube hole configuration and tube-to-tube sheet joint design within the limits of the essential variables of QW-288. The thickness of the tubesheet in the mockup test assembly shall be at least as thick as the production tubesheet, except it is not required to be thicker than 2 in. (50 mm). The mockup welds shall be submittedto the following tests sequentially and must meet the applicable acceptance criteria.

QW-193.1.1 Acceptance Criteria — Visual Examination.

QW-193.1.2 Acceptance Criteria — Liquid Penetrant.

QW-193.1.3 Acceptance Criteria — Macro‐Examination



From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Saravanan Sornam
Sent: Saturday, January 10, 2015 7:24 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:22700] tube to tubesheet welding

Dear venkatesh,
If your weld joint for tube to tubesheet is just a Seal weld and there is no special requirements from your client, then you can propose your client to use the existing pqr.
Check your client spec for any Mockups required as per ASME IX Qw193.
Is this for U stamp Project?
If yes, then you write a WPS based on existing 10 mm PQR , once it is confirmed as Seal Weld in your fab. Dwg
Seal weld is nothing but a fillet weld.
Read ASME QW 288 also for tube to tubewelds.
Regards
Sarav.

On Jan 10, 2015 12:00 AM, "venkkatesh krishnan" <venkkateshkrishnan@gmail.com> wrote:
Dear Sir,

            Thanks for your reply, code of construction is ASME SEC IX & SEC VIII DIV.1, and i have PQR qualified thickness is 10mm with 3G position,my doubt is to initiate the tube to tubesheet welding process before i need to do any Welder Performance Qualification Record(WPQ)?

            I am awaiting for your reply, Thanks in advance.

Regards,
Venkkatesh

On Thursday, January 8, 2015 at 11:17:26 PM UTC+5:30, Josnit wrote:
Hi,
What is the code of construction?
Considering welding code as Section IX and construction code Section Viii div. 1
If your PQR is qualified on 10mm plate in 3G, then both of ur tube as well as tubesheet, with range 1.5mm to 20mm. You can use it for welding tube to tubesheet welding. 

If your PQR thickness is less r more than 10mm then you may have to club it with any other PQR based on the ranges required.

Above info is valid only if construction code is ASME section VIII Div.1. If it is Div.2 then you have to qualify a pqr as per QW-193 of ASME section IX.

Hope above information is useful to you.

Sent from my iPhone

On Jan 8, 2015, at 19:09, venkkatesh krishnan <venkkates...@gmail.com> wrote:

Dear Experts,

             I need to do tube to tubesheet welding for CS Steel that is tubesheet material is SA 516 Gr.70 thk 20mm and tube material is SA 179 thk is 2.108mm welding process is GTAW, i have WPS in GTAW process with 3G welding my doubt is this WPS is suit for above mentioned statement or i need to qualify any welder qualification for welding this process. kindly please suggest me what ill do.


i am awaiting for your reply.

Thanks & Regards,

G.Venkkatesh.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/217c30f1-3ed9-4eb3-8a45-ad170f34246f%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/a03dc0f1-5492-45b3-aaf6-e4508542c4dd%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALV1rkLyqZ2Na--BCohe8cmz3GMAp%3Dx1jtk_96rD%2Bwnopj900Q%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...