RE: [MW:21135] Poke Mark observed in thin wire SAW

Hi Mohit ,
 
Please seethe attached paper on SAW , which gives a small hint to this problem. Also similar query was discussed in this forum earlier. Such uncharacteristic surface finish may happen with SAW fluxes containing lass  Ca-fluorides, which adds to fluidity of the flux.
 
Uneven grain size,  excess flux burden (flux feed) during ,delayed freezing all leads to this defect. Typically the flux burden, 1" or a little more, so as to generate, thin beads would not cause this problem. Again this problem may vary from flux to flux. You need to get flux manufacturer's recommendation also. What was the flux used in this case? You may reply in my personal email if you wish so.
 
Also see the earlier Q&A  on the same topic posted in this group.
 
Thanks
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
pradip_goswami@yahoo.ca
 

 

From: Prakash Hegde [mailto:pb.hegde@yahoo.com]
Sent: Saturday, June 14, 2014 10:52 AM
To: materials-welding@googlegroups.com
Cc: pgoswami
Subject: Re: [MW:21113] Poke Mark observed in thin wire SAW

Some time excessive Flux burden height also causes poke mark ,
lease check
i) Baking of Flux  and its temp (You may have to increase by about 25C than recomendation)
ii) Location of nozzle(Wire) on cirseam It should be about 25-50mm offset To maintain proper flux burden height
iv) Excessive current
Regards
Hegde P.B.


On Saturday, 14 June 2014 2:58 PM, Mahendra Arya <mkarya.delhi@gmail.com> wrote:


Kindly use baked flux....
On 14-Jun-2014 2:08 pm, "Mohit Aggarwal" <aggarwalmohit05@gmail.com> wrote:
>
> Respected Experts,,
> We are doing thin wire SAW ON Ss material pipe to pipe joint observing poke mark often. Kindly let me know how can it be eliminated because it effecting over all.productivity due to grinding of poke marks observed in weld metal layer!!
>
> Best Regards
> Mohit Aggarwal
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to mailto:materials-welding%2Bunsubscribe@googlegroups.com
> For more options, visit this group's bolg at http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>  
> The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an email to mailto:materials-welding%2Bunsubscribe@googlegroups.com.
> For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


No comments:

[MW:35738] ASME IX WPS Qualification Query: GTAW + FCAW with Multiple PQRs

Dear Welding Experts, I'm currently preparing a Welding Procedure Specification (WPS) and have encountered a request to qualify a GTAW +...