Skip to main content

Re: [MW:19626] Vacuum box test- API 650

BEGIN:VCARD
X-LOTUS-CHARSET:UTF-8
VERSION:3.0
PRODID:-//Lotus Development Corporation//NONSGML Notes 8.5.2//EN_C
FN:George H Dilintas/GRC/VERITAS
N:Dilintas;George;;;
ADR;TYPE=WORK;TYPE=PREF:PIRAEUS;;23\, Etolikoy Str.;PIRAEUS;;185 45
;GREECE
ADR;TYPE=HOME;TYPE=PREF:;;19-21 B. Laskou str.;Athens;Attika;11 633
;Greece
TEL;TYPE=HOME:+30-1-7667 197
TEL;TYPE=WORK:+30-210-40 63 113
TEL;TYPE=HOME;TYPE=FAX:+30 - 1 - 7667 197
TEL;TYPE=WORK;TYPE=FAX:+30-210-40 63 118
TEL;TYPE=CELL:+30 -69 44-64 62 04
EMAIL;TYPE=WORK;TYPE=PREF;TYPE=INTERNET
:george.dilintas@gr.bureauveritas.com
ORG:Bureau Veritas;Industry
REV:20131201T024559Z
END:VCARD

Vacuum Box is classified by ASME as an NDE Methode.
You may refer to ASME BPVC - Section V - Article 10, Mandatory Appendix II

    best regards

    Dr. Georgios Dilintas

    Authorized Nuclear Inspector
    Authorized Inspector Supervisor
    API 510 Inspector

    I&F REGIONAL TECHNICAL MANAGER
    BUREAU VERITAS HELLAS

    Tel: +30 210 40 63 113/4
    Fax: +30 210 40 63 118
    Cell: +30 69 44 64 62 04
    (See attached file: Dilintas_George.vcf)

"Kale, Bhaskar M" ---16/12/2013 08:44:22---Vacuum box leak testing is to locate leaks in a pressure boundary that cannot be directly pressurize

From: "Kale, Bhaskar M" <bmkale@gmail.com>
To: materials-welding@googlegroups.com
Date: 16/12/2013 08:44
Subject: Re: [MW:19624] Vacuum box test- API 650
Sent by: materials-welding@googlegroups.com




Vacuum box leak testing is to locate leaks in a pressure boundary that cannot be directly pressurized. Very minute leakage throughout the body (one side of wall to other side of wall) can check with vacuum box leak test.
LPT is locating the surface opening discontinuities only. And not giving the any idea if the discontinuity is throughout the body.
 
Both the methods have distinct benefits and can't say which one is superior. It's purely depends what type of discontinuity you are looking for; accordingly you may apply the method.
 
Regards,
Bhaskar



On Mon, Dec 16, 2013 at 1:57 PM, Kumar <sk7920541@gmail.com> wrote:




--
धन्यवाद,
भास्कर मनोहर काळे
+60149129098

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit
https://groups.google.com/groups/opt_out.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...