Skip to main content

Re: [MW:19617] Duplex UNS 31803 - FCAW Shielding Gas


Welding duplex material UNS 31803

TIG welding is usually performed with pure argon as the shielding gas. Resistance to, in particular, pitting corrosion can be considerably raised by the addition of up to 2% nitrogen. However, because the risk of pores  increases with increased nitrogen content, the latter should not exceed 2%. The addition of around 30% helium markedly increases arc energy and thus enables a considerable increase (20–30%) in welding speed. In the welding of duplex steels, the addition of hydrogen is not to be recommended. In combination with the high ferrite content (over 70%), this can lead to hydrogen embrittlement. Single-sided root beads must be welded with a backing gas. This is normally the same as the shielding gas.   A backing gas should also be used for tack welding all the way up until weld thickness is at least 8 mm.
 
FCAW is most suitably performed using argon with an addition of 16–25% carbon dioxide as the shielding gas. Welding with pure carbon dioxide is also possible, but arc stability and weld pool control are noticeably poorer. However, compared with a mixed gas, one advantage is that penetration is slightly better. Also compared with a mixed gas, the voltage should be increased by 2–3 volts when welding with pure carbon dioxide. This prevents the arc being too short.

Also enclosing filler wire details and  hope it will of help to you.


sridhar
 

 


From: Saravanan Sornam <saravanshyla@gmail.com>
To: materials-welding@googlegroups.com
Sent: Sunday, 15 December 2013 4:21 PM
Subject: [MW:19600] Duplex UNS 31803 - FCAW Shielding Gas

Dear Welding Experts ,

Could you please share quite urgently that,

which shielding gas is best applicable for FCAW-GS for welding Duplex material grade UNS 31803 ( P No. 10H ) and why ?

Also, share the best Preheat method for high alloy steels to remove moisture and for high thk joint applications .

Awaiting for your reply.

Thanks and Regards,
Saravanan,
Korea.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.


Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .