Friday, May 31, 2013

Re: [MW:17852] Welding and cladding SA-516 Gr. 60 + AISI 410S

Hi!
I would like to share my experience with 410S overlay on CS
i) If you try to overlay 410S/410  chemistry on Cs,  It does not pass in bend during bend test as per ASME sec IX (It cracks) if client is very stringent and he requires only 410S chemistry in such case you require to take waiver  for Bend test which is job specific
 
 You can try with 410 consumable with low C% less than 0.04 (Which is very difficult to get( Some time even 309MoL/309L barrier  with subsequent layer by 410 chemistry being used)
 
ii) Some time you may use 410 Ni Mo to get satisfactory bend test results However weld chemistry will have Ni ,Mo but major element will of Cr which will be in the range of 410
 
iii) However my experience is a) ",client accepts the 309L/309MoL for 410 clad restoration and b)  for high temp service (Like coke drum)client accepts the NiCrFe3 or NiCrMo3 chemistry where there is no problem of crack during bend test
 
In such case PWHT temp governs as per  UCS56 of ASME Sec VIII
Regards
 
Hegde P.B.
 
 
--- On Fri, 31/5/13, Ramin Kondori <raminkondori if clie@gmail.c would like tostry shareIom> wrote:s
ring bend test as
From: Ramin Kondori <raminkondori@gmail.com>
Subject: Re: [MW:17849] Welding and cladding SA-516 Gr. 60 + AISI 410S
To: materials-welding@googlegroups.com
Date: Friday, 31 May, 2013, 2:54 PM

410S itself is not martensite but this is when you have a weld metal
which is only consisted of 410S not mixture of carbon steel and
410S...

Dilution will occur and chemical analysis of the weld will be totally
different than 410S.

When 410S is deposited on carbon steels, depending on the carbon
content of the substrate, the resulted weld metal will be something
new rather than 410S...

Cr wil be around 6-8% and There will be martensite in resulted weld
metal. This martensite, if exceeds certain levels will be problematic
and should be avoided. Some references recommend a maximum of 30%
martensite in the weld metal microstructure and some allow up to 50%
martensite in the microstructure. This is only achievable by
preheat...

One safe method is to use a buffer layer such as 309L or 310 followed
by a low heat input process like Pulsed-MIG for depositing the 410 (or
410S if it is available) layer to avoid a layer which is over-alloyed
by Cr...

Depending on the client, this becomes a difficult task as the client
does not accept variations in Cr levels in top layer of overlay. So
clear every thing with the client or inspector before proceeding.

Regards
Ramin Kondori

On 5/30/13, c.nopadon@vipco-thai.com <c.nopadon@vipco-thai.com> wrote:
> My memory is stainless steel grade 410 is martensitic and suffix S is
> related to welding issue.
> Regards,
> C.Nopadon
>
> -----Original Message-----
> From: materials-welding@googlegroups.com
> [mailto:materials-welding@googlegroups.com] On Behalf Of kannayeram
> gnanapandithan
> Sent: Wednesday, May 29, 2013 12:29 PM
> To: materials-welding@googlegroups.com
> Subject: Re: [MW:17828] Welding and cladding SA-516 Gr. 60 + AISI 410S
>
>  SS 410S is not martensitic
>
> On 5/28/13, Ramin Kondori <raminkondori@gmail.com> wrote:
>> *Dear Branko:*
>>
>> Depositing AISI 410S on A516 will produce a martensitic weld overlay
>> which is prone to cracking even during welding. There Are two solutions:
>>
>>    1. Using a buffer layer (intermediate layer) of E309L or even E310L on
>>    A516 and then Depositing 410S
>>    2. Applying preheat of min 250-300 C which makes it a very hard job
>>    though it may seem less expensive
>>
>> In first scenario, you do not need any preheat but I do not recommend
>> using SAW for 410S layer since it may melt through the buffer layer
>> and reach
>> A516 which maybe, maybe causes problems. You can use GMAW with Ar+2%o2
>> or
>> Ar+3%CO2. Do not forget the Preheat...
>>
>> This way your weld overlay will be thicker than 3 mm and you should
>> weld a PQR coupon to make sure you have 3mm of 410 weld layer "over"
>> the buffer layer. Maybe you'll have to deposit one buffer (309L or
>> 310L) and 2 layers of 410S. Try using Pulsed GMAW to get the results
>> with depositing one layer.
>>
>> One of our colleagues have successfully deposited one layer of 410
>> weld overlay on A516 using Pulsed-MIG (Preheat is essential). It's
>> because Pulsed-MIG has less dilution and you may achieve required
>> results in one layer.
>>
>> For PQR, you need 4 side bend tests, chemical analysis on the surface
>> of overlay and 3-4mm below the surface, and hardness test (on the
> surface).
>>
>> Discuss these issues with your client before proceeding.
>> Good Luck
>> *Ramin Kondori*
>> *Sr. QA/QC Engineer
>> *
>> *SINOPEC*
>>
>> r.kondori@petroyada.com
>> +98-2123592322
>> +98-9132150320
>>
>>
>> On Mon, May 27, 2013 at 4:37 PM, Branko Ferencak <bran2605@gmail.com>
>> wrote:
>>
>>> I have shell 20mm thick ( SA-516 Gr, 60 ) and there must be cladd
>>> AISI 410S 3mm Could anybody tell me which filler i can use, for SAW
>>> and GMAW?
>>> GMAW i  planning use for flanges and tubesheets ( after i overlay
>>> tubesheet - what is procedure for welding tube to tubesheet? ) Also
>>> PWHT has been asked by customer after overlay.
>>> Can anybody tell the effect of PWHT on SS 410S overlay?
>>> What will be the the safe range of temperature of PWHT?  ( Also
>>> recommended temperatures and times, holding cooling...)
>>>
>>> Best regards,
>>> Branko Ferencak
>>>
>>>  --
>>> To post to this group, send email to
>>> materials-welding@googlegroups.com
>>> To unsubscribe from this group, send email to
>>> materials-welding+unsubscribe@googlegroups.com
>>> For more options, visit this group's bolg at
>>> http://materials-welding.blogspot.com/
>>>
>>> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=1227
>>> 87&trk=anet_ug_hm
>>>
>>> The views expressed/exchnaged in this group are members personel
>>> views and meant for educational purposes only, Users must take their
>>> own decisions w.r.t. applicable code/standard/contract documents.
>>> ---
>>> You received this message because you are subscribed to the Google
>>> Groups "Materials & Welding" group.
>>> To unsubscribe from this group and stop receiving emails from it,
>>> send an email to materials-welding+unsubscribe@googlegroups.com.
>>> For more options, visit https://groups.google.com/groups/opt_out.
>>>
>>>
>>>
>>
>> --
>> To post to this group, send email to
>> materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=12278
>> 7&trk=anet_ug_hm
>>
>> The views expressed/exchnaged in this group are members personel views
>> and meant for educational purposes only, Users must take their own
>> decisions w.r.t. applicable code/standard/contract documents.
>> ---
>> You received this message because you are subscribed to the Google
>> Groups "Materials & Welding" group.
>> To unsubscribe from this group and stop receiving emails from it, send
>> an email to materials-welding+unsubscribe@googlegroups.com.
>> For more options, visit https://groups.google.com/groups/opt_out.
>>
>>
>>
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=
> anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups
> "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an
> email to materials-welding+unsubscribe@googlegroups.com.
> For more options, visit https://groups.google.com/groups/opt_out.
>
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups
> "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an
> email to materials-welding+unsubscribe@googlegroups.com.
> For more options, visit https://groups.google.com/groups/opt_out.
>
>
>


--
*Ramin Kondori*
*Sr. QA/QC Engineer
*
*SINOPEC*

r.kondori@petroyada.com
+98-2123592322
+98-9132150320

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...