Hi,
Austenitic stainless steels with around 10-12% nickel (e.g. grades 304, 316, 321 and 347) are predominantly non-magnetic due to the face centred cubic (fcc) crystal structure of the austenite phase, which imparts so-called 'paramagnetic' (i.e. non-magnetic) behaviour.

Although a number of second phases, e.g. inclusions or ferrite stringers, may exist in wrought austenitic stainless steel products, the structure is almost exclusively made up of the austenite phase and hence they are essentially non-magnetic. However, weld metals made with filler metal compositions matching the 300 series austenitic steels (e.g. 308, 309, 316 and 347 types) are designed to have a small fraction of delta ferrite phase, typically around 5-15%, to reduce significantly the risk of solidification cracking, which exists for purely austenitic compositions. The delta ferrite phase has a body centred cubic (bcc) structure, which has 'ferromagnetic' properties (i.e. typical magnetic properties, as associated with, for example, mild steels, carbon steels and low alloy steels).

Some delta ferrite may form also in autogenous weld metal (i.e. parent metal which is fused without filler metal addition) and the high temperature heat affected zone of a weld, where partial transformation to delta ferrite can occur on heating and where cooling is too rapid for full re-transformation. Hence, overall, welds in many of the 300 series austenitic stainless steels, made with no filler or approximately matching filler will typically show mildly magnetic properties.

Some higher alloyed austenitic steels, with significantly more than 12% nickel, such as type 310, do not show such magnetism as they have a stable, fully-austenitic structure as a result of the high level of nickel, which stabilises the fcc structure in preference to bcc. Resistance to solidification cracking is then achieved by adding manganese to the filler metal and keeping impurity levels to a minimum.

Where low magnetic permeability is a desirable property for welds in common 300 series steels, welding filler metal should be chosen to give very low ferrite levels. Type 310 is an option and 'nil-ferrite' 316 types are available.

Thanks : TWI

Palanivelan.V

On May 28, 2013 10:47 PM, "guru vasanth" <guruvasanth@gmail.com> wrote:
Dears experts,

Could you explain the reason of 300 series Stainless steel magnetization after welding?

Thanks

Regards

Guru S Mahalingam

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...