Hi,
Perhaps you are refeering to Solution Annealing (Annealing the weldment @ 1038 degC, followed by water quench)in order to eliminate Carbide precipitation but this is an expensive and impractical procedure, So if weldments operate in sever corrosive environments or within the sensitization range,either extra low carbon grades (E304L, E308L) or stabilized grades are needed.
Regards
Manpreet Singh
Dear Experts,
Is it advisable to water quench the Austenitic S.S. PQR (6 mm. Base Metal Thk., SA 240 Tp. 316L) subsequently after each pass and before proceeding for next pass?
Same procedure was followed during PQR of 6 mm. to 10 mm. base metal Thk. SA 240 Tp. 304L PQR to control the inter pass temp. max. 100º C. But, unfortunately, the PQR was failed in IGC test as per ASTM A 262 Pr. E. Intermetallic ditches observed in weld metal, and in H.A.Z. and Parent Metal- Ditch structure observed. Also one root bend was failed in testing. What will be the reason?
Which precautions to be taken during qualification of 6 mm. Base Metal Thk., SA 240 Tp. 316L PQR and what will be the qualified max. range of base metal thickness?
Please share your experience with me.
Thanks & regards,
C. R. GANDHI
(Welding Engineer)
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Perhaps you are refeering to Solution Annealing (Annealing the weldment @ 1038 degC, followed by water quench)in order to eliminate Carbide precipitation but this is an expensive and impractical procedure, So if weldments operate in sever corrosive environments or within the sensitization range,either extra low carbon grades (E304L, E308L) or stabilized grades are needed.
Regards
Manpreet Singh
Dear Experts,
Is it advisable to water quench the Austenitic S.S. PQR (6 mm. Base Metal Thk., SA 240 Tp. 316L) subsequently after each pass and before proceeding for next pass?
Same procedure was followed during PQR of 6 mm. to 10 mm. base metal Thk. SA 240 Tp. 304L PQR to control the inter pass temp. max. 100º C. But, unfortunately, the PQR was failed in IGC test as per ASTM A 262 Pr. E. Intermetallic ditches observed in weld metal, and in H.A.Z. and Parent Metal- Ditch structure observed. Also one root bend was failed in testing. What will be the reason?
Which precautions to be taken during qualification of 6 mm. Base Metal Thk., SA 240 Tp. 316L PQR and what will be the qualified max. range of base metal thickness?
Please share your experience with me.
Thanks & regards,
C. R. GANDHI
(Welding Engineer)
| Follow Rediff Deal ho jaye! to get exciting offers in your city everyday. |
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Comments