Skip to main content

RE: [MW:13951] Backing strip

Please check your client specification.

Some of the equipments in petrochemical / refinery / Power services specify that no backing strip shall be used.

 

Prakash Raman .B

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of prem nautiyal
Sent: Tuesday, March 20, 2012 2:48 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:13945] Backing strip

 


As i have mentioned earlier, the joint is a closing seam with no access from other side, hence can't be welded from inside.

Also the contractor does not want to take risk of any RT repairs with his qualified welders by welding a single sided FPW.

 

However as the root run and hot pass are going to be welded with TIG , there will be no chances of slag entrapment in root run between metal backing strip and shell/dishend.

 

Considering Spot radiography as per UW-12, the issue is now cleared.

 

Regards

 

Prem Nautiyal


--- On Tue, 3/20/12, gopunair5343@yahoo.com <gopunair5343@yahoo.com> wrote:


From: gopunair5343@yahoo.com <gopunair5343@yahoo.com>
Subject: Re: [MW:13943] Backing strip
To: materials-welding@googlegroups.com
Date: Tuesday, March 20, 2012, 2:03 PM

ASME Second VIII Div 1 permits use of backing strip for the type of joint in question. Please refer para UW-12 for joint efficiency.

But why the contractor is not prefering a single side full penetration joint configuation or even a double welded butt joint. Welding from inside is not a big issue for 600 dia shell.

RT with backing strip in position may be a bit tricky and interpretation problematic due to slag entrapment between shell and b/s.

Gopu

Sent from BlackBerry® on Airtel


From: prem nautiyal <prem_nautiyal26@yahoo.com>

Sender: materials-welding@googlegroups.com

Date: Tue, 20 Mar 2012 00:19:33 -0700 (PDT)

To: <materials-welding@googlegroups.com>

ReplyTo: materials-welding@googlegroups.com

Subject: [MW:13932] Backing strip

 

Hello friends

 

Need expert opinion on the subject as follows..

 

A Heat exchanger is being fabricated as per ASME Sec VIII Div.1.

The Channel Shell and dish end thickness is @ 10mm and dia. @ 600mm. The MOC is SA516 Gr.70.

Now for the closing joint seam i.e. Channel Shell # Dish end (single V joint) can a "Permanent Backing strip" with 8mm root gap be used ? The permanent backing strip will be 6mm thicknes X 25mm wide and stich fillet welded from inside. Contractor has submitted WPS mentioning permanent backing strip for this joint. Can we accept this ? Is there any provision in code for non-usage of permanent backing strips in pressure parts ?

The joint calls for full radiography. Contractor claims that upto 10mm thickness the RT will be cleared.

Can we accept this case as per ASME Sec.VIII Div.1.

 

Regards

 

Prem Nautiyal

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...