Skip to main content

Re: [MW:13991] PWHT OF P91 BY INDUCTION HEATING

Dear Mani/Balaji,
 
This was a demonstration of PHWT which we are going to follow on jobs,so client is not allowing to put wool inside.They want PHWT demo in the same manner ,which we are going to do on jobs. We had put metal dummy on both sides but no wool or coil.This is thermal power plant project and the acceptance codes are ASME sec I & ASME B31.1
 
Thanks &Regards
 
Sandeep.M.V
QC Engineer
On Mon, Mar 26, 2012 at 1:43 PM, E.S.Mani <maniesbk@gmail.com> wrote:

Dear sandeep,

 

Ya this is not acceptable. Because the temperature difference range is 732 Deg, C to 774 Deg C for P15E material as per B31.3 (2010 Edition).

 

I have understood from your mail, there is access to put the thermocouple means you can put more thermo wool to with stand the heat & start to monitor the temperature recorder, still it is coming down try to put more wool & dummy on both sides.


Regards,

E.Subramanian/Balaji.R


On Sun, Mar 25, 2012 at 12:04 AM, Harish Kannepalli <harishkannepalli@gmail.com> wrote:
Dear sandeep,
                 Please try putting coil inside the pipe also. As per code more than 60°C difference is not allowed.


2012/3/24 sandeep monody <smv.monody@gmail.com>
Dear experts,
 
In my site we conducted a demonstration of PWHT on SA335 P91 material (OD-450mm X 70mm Thk) as our clients requirement and details as given below.
 
Heating/cooilng rate;-60 deg C,Holding temparature:-760deg C and holding time:-180minutes,Heating band width:-210mm and insulation band width 630mm,Heating method :-Induction heating
 
During pwht we observed a temparature difference on outside and inside of pipe more than 80 deg C.
 
Now problem is that client is not accepting this method and asking for uniform temparature in outside and inside of pipe.
 
How can i control temparature at both sides?
Is it possible a uniform temp on both side with induction heating?
 
Please give ur valueble advice in this matter.
 
 
Sandeep.
QC Engr

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
regards,
Harish.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--

Regards,

E.Subramanian


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...