RE: [MW:10678] Titanium to carbon steel welding

Hello Vijay,
 
It's not very clear from the details posted, what's the thickness of the shell. For a heat exchanger involving corrosive fluid typically the wetted surface would be of Titanium.From that aspect Titanium clad carbon or low alloy steel looks to be the ideal cost effective material. However if the clients' choice is pure titanium then one has little choice. However the welding difficulties involved in for Titanium clad steels are lot less than solid titanium.
 
Under the present scenario, since the shell would be of pure titanium I would think the following could be the options for saddles:-
  1. Get the entire saddles fabricated from Titanium(as proposed by you).In reality one does not need Titanium saddles, but the design would drive towards the same and this would add up to the cost.
  2. or
  3. Get the saddles fabricated from Ti Clad steels-preferably explosion or roll bonded plates.
Titanium can not be arc welded to Carbon steel due to formation of brittle intermetallic phases.
 
The attached articles would help to provide you some guidance on the welding problems of Ti and Tiitanium Clad steels.
 
Thanks.
 
 
Pradip Goswami,P.Eng.IWE
Welding & Metallurgical Specialist & Consultant
Ontario,Canada.
Email-pgoswami@sympatico.ca,
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Norton, Seth J
Sent: Thursday, April 14, 2011 9:52 AM
To: materials-welding@googlegroups.com
Subject: RE: [MW:10676] Titanium to carbon steel welding

Titanium and steel form brittle intermetallics and can not be joined by standard fusion welding processes. The only welding process I am aware of for joining steel and titanium is explosion cladding.

 

Seth Norton


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Prakash Hegde
Sent: Wednesday, April 13, 2011 10:35 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:10671] Titanium to carbon steel welding

 

You have to bearin mind the cost of Ti which is very very costly

 


From: vijay <vijayakumarme@gmail.com>
To: materials-welding@googlegroups.com; weldinggang@googlegroups.com
Sent: Thu, 14 April, 2011 5:25:58 AM
Subject: Re: [MW:10669] Titanium to carbon steel welding

Dear  Schreedhar/ Rizal/ Shaunak Upadhyay / Prakash Hegde,


Thanks for your valuable suggestions.

The saddle length is 200mm only, and I have suggested to use Titanium for the saddle to avoid dissimilar welding.

I think this will be the better decision to avoid carbonsteel to titanium welding problem.

 

Thanks and Regards,

Vijay

 

 


,

On Tue, Apr 12, 2011 at 1:06 PM, Prakash Hegde <pb.hegde@yahoo.com> wrote:

Dear Vijay

 

Ti To  Cs welding is not compatable

Generally  Ti lining (sheet ) is being screwed with CS, You  can refer AWS welding Hand book Vol 4 for the joint configuration Which will  clear your doubts

Regards

 

Hegde P.B.

 


From: vijay <vijayakumarme@gmail.com>
To: weldinggang@googlegroups.com; materials-welding@googlegroups.com
Sent: Tue, 12 April, 2011 6:09:13 AM
Subject: [MW:10646] Titanium to carbon steel welding

 

Dear Friends,

 

There is a requirement mentioned in our client spec about Titanium to Carbon steel welding(Attached picture have more details).

I searched for literatures on this and I found that by normal fusion welding process is not recommended.

1. Is there any way,welding can be done between Titanium and carbon steel?

2. If YES or NO(on both case), please send a evidence document to confirm(like ASME,ASTM).

This is very urgent requirement.

 

Thanks in advance

 

Regards,

Vijay

--

To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.