Yes, You can use ASTM materials qualified PQR for ASME materials
welding.

No restrictions as per ASME sec VIII Div-1 (Refer QW-28) or ASME Sec-
IX(Refer QW-420).

"If an unlisted base metal has the same UNS number designation as a
base metal listed in table QW/QB-422,
it shall be considered as assigned to that P-Number or P-Number plus
Group Number. However, only base metals listed in table QW/QB-422 with
minimum tensile strength values may be used for procedure
qualification test coupons".

Cheers!

Raj


On Apr 18, 7:57 am, Vino Varghese <vinopvargh...@gmail.com> wrote:
> Dear Raj,
>
> Thanks for the information, but still the query is not answered.
>
> *There is no Impact Test requirement for our Vessel.*
>
> Now can you please guide, whether i can prepare a WPS with an ASTM Material.
>
> Thanks & Regards
> Vino-Doha, Qatar
> ________________________________________________________________________
>
>
>
> On Mon, Apr 18, 2011 at 7:34 AM, Raj <raj.inspect...@gmail.com> wrote:
> > Hi,
>
> > Please refer UG-84(h)(2) of ASME Sec VIII Div.1'Ed'2010.
>
> > If impact testing is required in weld & HAZ when required by UCS-67,
> > the following shall apply.
>
> > For vessels constructed to the rules of part UCS, the test plate
> > material shall sitisfy all of the following requirements relative to
> > the material to be used in production.
>
> > (a) be of the same P-Number and Group Number;
> > (b) be in the same heat treated condition; and
> > (c) meet the minimum notch toughness requirements of UG-84(c)
> > (4) .......................
>
> > Means, one way or other, If you are using LTCS material for production
> > and requires notch touchness of weld and HAZ then the base material
> > used for Procedure shall be of same P No..(You can use ASTM A333 Gr.
> > 6(P1G1) to ASTM A350LF2(P1G2) procedure) but you can not use ASTM A106
> > Gr.B even though it is P1G1 since it "is not the same heat treated
> > condition" as that of A333 gr.6.
>
> > Hope this will clarify!
>
> > Cheers!
>
> > Raj
>
> > On Apr 17, 4:37 pm, Vino Varghese <vinopvargh...@gmail.com> wrote:
> > > Dear All,
>
> > > Design Code: ASME Sec VIII, Div 1
> > > U-Stamp Pressure Vessel
>
> > > Reference Code : ASME Sec IX, Edition 2007, Add 09
> > > Material of Construction: SA 516 Gr 70N(30mm thk)
> > > PQR Material : *1. Pipe* - ASME SA 333 and *2. Flange* : ASTM A350 LF2
>
> > > *Query:*
> > > *Is it mandatory that Qualification has to be done only with a ASME
> > > Material? *
> > > *If ASTM Material is used for qualification, then WPS will be qualified
> > only
> > > for that particualr Material and cannot be Qualified as P1 Material.
> > Please
> > > provide all reference from Code for justification*.
>
> > > Hope to see that i was able to communicate properly with regard to raised
> > > query.
>
> > > Expecting as usual response from all sides.
>
> > > Thanks & Regards
> > > Vino-Doha
>
> >  --
> > To post to this group, send email to materials-welding@googlegroups.com
> > To unsubscribe from this group, send email to
> > materials-welding+unsubscribe@googlegroups.com
> > For more options, visit this group's bolg at
> >http://materials-welding.blogspot.com/
> > The views expressed/exchnaged in this group are members personel views and
> > meant for educational purposes only, Users must take their own decisions
> > w.r.t. applicable code/standard/contract documents.- Hide quoted text -
>
> - Show quoted text -

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...