Friday, February 11, 2011

RE: [MW:9822] SA 516 Gr.60 high in manganese-accept or reject

Refer the note B of Table 1 in SA516

“For each reduction of 0.01 percentage point below the specified maximum for carton, an increase of 0.06 percentage point above the specified maximum for manganese is permitted, up to a maximum of 1.50% by heat analysis and 1.60% by product analysis”.

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of krishna
Sent: Friday, February 11, 2011 5:02 PM
To: materialswelding
Subject: [MW:9821] SA 516 Gr.60 high in manganese-accept or reject

 

Dear all,
                  We have received MTC for SA 516 Gr.60 plate of 10mm thickness with manganese of 1.47%,the lab test also give the same.

is it acceptable as per SA 516 SPEC.

Please confirm shall we accept or reject the plates,we have procured more tonnes of materails & started fabrication?

what shall we do in this stage?

How to overcome this issue ,pls guide

krishna