Mr. Zakaria,
 
Attached are some information on Corten Steel/Weathering Steel which would be of help to you. This steel is a micro alloyed, typically added with Copper (major) and other alloying elements, such as Nickel to improve atmospheric corrosion resistance.
 
ASTM A-588 is one of the specifications which cover such (weathering) steel. See the attached data sheets for  further references.
 
Corten is quite weldable, with the required precautions to be adopted as per manufacturers guidelines.
 
AWS SFA 5.5 covers the required specs for welding electrodes,recommended electrodes are E-7018W for Corten A, E-8018W for Corten-B steel.See the atatched data sheet of a popular electrode manufacturer in North America, Air Liquide.
 
ASME Sec-IX  includes weathering steel, under specification A-588. These steels have S-Nos but do not have any P No.Welding procedure qualification on these ASTM specification specific. PQR  qualified for  these steels apply for welding these grades or to others. It's advisable to use welding electrodes matching the Corten chemistry for welding dissimilar materials.
 
What's  grade or specification of corten to be fabricated. If you specify more details , perhaps may get more appropriate guidelines.
 
Thanks.
 
 
Pradip Goswami,P.Eng.IWE
Welding & Metallurgical Specialist & Consultant
Ontario,Canada.
Email-pgoswami@sympatico.ca,
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of muthusrinivasan muthuselvam
Sent: Thursday, February 24, 2011 1:30 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:10007] Corten & carbon Steel weldability

Carton steel is microalloyed carbon steel material mainly used for weathering action.. basically this material is developed for special application... in India equvalent material is IRSM 41-- If you check the chemistry and mechanical in internet you will get it..

On Sat, Feb 19, 2011 at 12:33 PM, k.ilangkumaran ilangkumaran <k.ilangkumaran@yahoo.com> wrote:
Dear MSMS,
 
               E7018 W? How? could you please explain us? because the material is unassigned as mentioned so we dont know what chemical composition and tensile strength is? some standards para if possible please?
 
Ilan

--- On Fri, 2/18/11, muthusrinivasan muthuselvam <msms2k@gmail.com> wrote:

From: muthusrinivasan muthuselvam <msms2k@gmail.com>
Subject: Re: [MW:9922] Corten & carbon Steel weldability Date: Friday, February 18, 2011, 3:32 PM


Dear Mr.Zakaria..
 
Corten is unspecified material as per ASME... you can say that as unassigned and preferred electrode is E 7018 W -made to order.
 
I hope this is for chimney or some container..
 
br,
 
msms

On Thu, Feb 17, 2011 at 9:14 PM, Zakaria ghrab <zakaria.ghrab@gmail.com> wrote:
Hi all,

  I need to know the P number of corten steels, i have on PQR according ASME sect IX corten to corten, i need to use it to prepare WPS for Carbon steels but i have doute Corten is PN°1 or PN°3, serashing in internet : Equivalent Corten is ASTM SA 242, is it true?
--
GHRAB Zakaria
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...