Welding of Hastealloy C22
 
Suitable Process : GTAW (Root+ Next PASS)
                            SMAW : Rest
 
Joint Detail : Single Vee, Bevel Included angle 60-75 degC,Root opening 0.8-4.0mm, Root Face : 0.8-2.4 mm
 
Welding consumable GTAW : ER NiCrMo-10
                                SMAW : E NiCrMo-10
 
Preconditioning of SMAW electrodes : As per Manufacturer Recommendations
 
PreHeat : Room Temperature
Interpass : 93degC maximum
 
Joint Cleanliness is Imporatnt.

J.GERALD JAYAKUMAR
00919344954677
 


--- On Wed, 2/23/11, vijay <vijayakumarme@gmail.com> wrote:

From: vijay <vijayakumarme@gmail.com>
Subject: [MW:9996] Need advice on Hastelloy C22.
To: materials-welding@googlegroups.com
Date: Wednesday, February 23, 2011, 11:36 PM

Dear Friends,

 

I need technical advice to go with Welding on Hastelloy C22 (SB 575, UNS N06022). The maximum thickness of the plate is 12mm and the code as per ASME IX. This requirement is for Gas&Condensate cooler for a offshore platform project.


Thanks & Regards,

Vijay

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...