Skip to main content

RE: [MW:9609] heat input calculation in welding

From an ASME Section IX Code stand point the below statements are not correct.

 

On should read the Section IX, QW-409.1, interpretations (there are quite a few).  In particular one should Interpretation IX-81-91.  However, I will transcribe portions of several interpretations that are interesting:

 

IX-81-19

Q4 – ā€œIf QW-409.1 does not require that average heat input be determinedā€ {previous question – reply No} ā€œhow is heat input established for multiple pass procedure qualification?  Must it be established for each pass?

R4 – QW-409.1 requires requalification when an increase in heat input occurs over that qualified.  Maximum heat input is established during procedure qualification by determination of the maximum amperage and voltage in combination with the least travel speed or, alternatively, the maxi mum volume of weld metal deposited per unit length of weld.  Heat input is not required to be determined for each pass.

 

IX-04-12

Q1 – Does QW-409.1 require the highest heat input, to be recorded on the PQR, be calculated on the parameter used at the location where the HAZ impact specimens are removed.

R1 – No.

 

Although, I will admit I record amperage, voltage, and travel speed for each pass when performing PQR welding whether impact testing is required or not;  i.e. whether QW-409.1 is an essential variable or not applicable.

 

John

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Pablo J Acelajado
Sent: Friday, January 28, 2011 2:16 AM
To: materials-welding@googlegroups.com
Subject: RE: [MW:9541] heat input calculation in welding

 

January 28, 2011

 

Hello!

 

You need to show the individual Heat input of each pass and also indicate the sum or total Heat input. 

 

Thanks & best regards.

 

PJA


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of manpreet
Sent: Friday, January 28, 2011 9:55 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:9538] heat input calculation in welding

 

Dear Sandeep,

As stated by you that "every pass has its effect on base metal", Your PQR shall include heat input for each pass and WPS to be written with Heat Input for each pass, as per QW-409.1, any increase in heat input for each pass will require requalification.

Heat input shall be calculated with QW-409.1 (a) and (b), if with any of these methods Heat Input is increased, you need to requalify the WPS, that's why max. heat input value is written for WPS.


Regards
Manpreet Singh




On Fri, 28 Jan 2011 10:55:51 +0530 sandy wrote
>Hi everybody
>
>I have one query regarding the heat input.
>If I am welding a joint with multipass, then I have diffrent heat
>input for every pass depening on the parameters. now I want to know
>which heat input shall be taken into consideration for the effect of
>heat input on base metal, cauz every pass has its effect on base metal
>and after every pass due to the previous heat input I am giving extra
>heat in the base metal.
>So I want to know should I take individual heat input or sum of all
>heat input for getting the exact effect of Heat input on base metal.
>
>Regards
>Sandeep Kumar
>
>--
>To post to this group, send email to materials-welding@googlegroups.com
>To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...