Friday, August 31, 2012

Re: [MW:15176] Defects in the MIG welding of F91+F91 -reg

It is not a matter of shielding gas. Try to keep the arc shorter (lower volts) and remove the torch very slowly
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager


  From: Sankaran Sp [subasankaran@yahoo.co.in]
  Sent: 31/08/2012 18:03 ZE8
  To: materials-welding@googlegroups.com
  Subject: [MW:15173] Defects in the MIG welding of F91+F91 -reg


Dear friends,

I am working the leading valve manufacturing company in Coimbatore ( INDIA) i ma facing quality issue in the MIG welding of Er 90S-B9.
We have product in ASTM A182- F91 forged steel valve ( Equivalent to C12A casting or P91 pipes),during welding of body+Bonnet we are facing the crack in the crater area.
Our welding parameters are as below:
Joint type = Circumferential Fillet welding, Current = 215 - 235  Amps, V = 25 - 27 Volts, Shielding Gas = Ar+CO2 ( 80+20 % mixture), Gas flow = 20 - 25 LPM, Pre heat temp =  210 - 230 Deg C, Inter pass temp= 320 - 380 Deg C
>After welding ,the joint was inspected by M.P test andcrack found on crater area.
> Removed the welding by turning, then re- test carried out with increased
the post flow timings of shielding gas, but no improvement in the test, same
crack appeared on crater area.

What will be the reason for this defect? Can you suggest me suitable method
to over come this problem?
What will be the reason for this crack?
Kindly send your recommendations to solve this issue.

Advance thanks and regards,
Sankaran.SP
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 
~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~
NOTICE: This message contains information which is confidential and the copyright of our company or a third party. If you are not the intended recipient of this message please delete it and destroy all copies. If you
are the intended recipient of this message you should not disclose or distribute this message to third parties without the consent of our company. Our company does not represent, warrant and/or guarantee that the integrity of this message has been maintained nor that the communication is free of virus, interception or interference. The liability of our company is limited by our General Conditions of Services.
Nota : Ce message contient des informations confidentielles propriété de notre société et/ou d'un tiers. Si vous n'êtes pas parmi les destinataires désignés de ce message, merci de l'effacer ainsi que toutes ses copies. Si vous êtes parmi les destinataires désignés de ce message, prière de ne pas le divulguer ni de le transmettre à des tiers sans l'accord de notre société. Notre société ne peut garantir que l'intégrité de ce message a été préservée ni que la présente communication est sans virus, interception ou interférence. La responsabilité de notre société est limitée par nos Conditions Générales de Services.
~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~~

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

RE: [MW:15175] Invitation to IIW Monthly Technical Lecture_31st Aug 2012 @ Mumbai, India

Good morning sir,
Requested to send mail in advance at least week time . I am interested for the same.

Regards,
RK Vichare
(M)9869679123



 
----- Original Message -----
From: Mistry K.U (Mumbai - Construction)
To: materials-welding@googlegroups.com
Sent: Fri, 31 Aug 2012 14:26:23 +0530 (IST)
Subject: RE: [MW:15172] Invitation to IIW Monthly Technical Lecture_31st Aug 2012 @ Mumbai, India









Too late info  - please arrange such info in little advance please.


 


K. U. Mistry


Manager QA/QC


Tecnimont ICB Pvt Ltd


LLDPE/HDPE (SWING) Project


OPAL Dahej Off Shore Project Site Gujarat


 



From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com]
On Behalf Of prem nautiyal

Sent: 31 August 2012 11:48

To: materials-welding@googlegroups.com

Subject: [MW:15170] Invitation to IIW Monthly Technical Lecture_31st Aug 2012 @ Mumbai, India



 









 


 









 





 


Dear All,



Indian Institute of Welding, Mumbai branch cordially invites you for a technical lecture on



"Welding Requirements for Offshore Oil & Gas Projects"



By Mr. Maruti Kumar, AEE(E) / Mr. D. Badole, CE(M) / Mr Pradeep N. Nair, CE(E) From :QA
& Vendor Cell, Offshore Engineering Services, ONGC, Mumbai, India.


On Friday, 31-08-2012 at 6.15 pm



At


Avion Hotel,


Domestic Airport, Nehru Road, Vile Parle (East), Mumbai - 400 057, India.


Mumbai Branch Tel No : (022) 25772637


Tel: (022) 25772637


Refer attached file for more details.




Regards,


 



Prem Nautiyal




The Indian Institute Of Welding




Mumbai Branch




Cell: 9769316004





 















--


To post to this group, send email to materials-welding@googlegroups.com

To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com

For more options, visit this group's bolg at
http://materials-welding.blogspot.com/


http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

 

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

 








--

To post to this group, send email to materials-welding@googlegroups.com

To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/

http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

 

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

 


Re: [MW:15174] Invitation to IIW Monthly Technical Lecture_31st Aug 2012 @ Mumbai, India

Is there any program in gulf? Please update.

Regards,

Syed Mazhar Ali


From: prem nautiyal <prem_nautiyal26@yahoo.com>
To: materials-welding@googlegroups.com
Sent: Thursday, 30 August 2012, 20:11
Subject: [MW:15170] Invitation to IIW Monthly Technical Lecture_31st Aug 2012 @ Mumbai, India






Dear All,
Indian Institute of Welding, Mumbai branch cordially invites you for a technical lecture on
"Welding Requirements for Offshore Oil & Gas Projects"
By Mr. Maruti Kumar, AEE(E) / Mr. D. Badole, CE(M) / Mr Pradeep N. Nair, CE(E) From :QA & Vendor Cell, Offshore Engineering Services, ONGC, Mumbai, India.
On Friday, 31-08-2012 at 6.15 pm

At
Avion Hotel,
Domestic Airport, Nehru Road, Vile Parle (East), Mumbai - 400 057, India.
Mumbai Branch Tel No : (022) 25772637
Tel: (022) 25772637
Refer attached file for more details.

Regards,
 
Prem Nautiyal
The Indian Institute Of Welding
Mumbai Branch
Cell: 9769316004
 


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 


[MW:15173] Defects in the MIG welding of F91+F91 -reg

Dear friends,

I am working the leading valve manufacturing company in Coimbatore ( INDIA) i ma facing quality issue in the MIG welding of Er 90S-B9.
We have product in ASTM A182- F91 forged steel valve ( Equivalent to C12A casting or P91 pipes),during welding of body+Bonnet we are facing the crack in the crater area.
Our welding parameters are as below:
Joint type = Circumferential Fillet welding, Current = 215 - 235  Amps, V = 25 - 27 Volts, Shielding Gas = Ar+CO2 ( 80+20 % mixture), Gas flow = 20 - 25 LPM, Pre heat temp =  210 - 230 Deg C, Inter pass temp= 320 - 380 Deg C
>After welding ,the joint was inspected by M.P test andcrack found on crater area.
> Removed the welding by turning, then re- test carried out with increased
the post flow timings of shielding gas, but no improvement in the test, same
crack appeared on crater area.

What will be the reason for this defect? Can you suggest me suitable method
to over come this problem?
What will be the reason for this crack?
Kindly send your recommendations to solve this issue.

Advance thanks and regards,
Sankaran.SP
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

RE: [MW:15172] Invitation to IIW Monthly Technical Lecture_31st Aug 2012 @ Mumbai, India

Too late info  - please arrange such info in little advance please.

 

K. U. Mistry

Manager QA/QC

Tecnimont ICB Pvt Ltd

LLDPE/HDPE (SWING) Project

OPAL Dahej Off Shore Project Site Gujarat

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of prem nautiyal
Sent: 31 August 2012 11:48
To: materials-welding@googlegroups.com
Subject: [MW:15170] Invitation to IIW Monthly Technical Lecture_31st Aug 2012 @ Mumbai, India

 

 

 

 

 

Dear All,

Indian Institute of Welding, Mumbai branch cordially invites you for a technical lecture on

Welding Requirements for Offshore Oil & Gas Projects”

By Mr. Maruti Kumar, AEE(E) / Mr. D. Badole, CE(M) / Mr Pradeep N. Nair, CE(E) From :QA & Vendor Cell, Offshore Engineering Services, ONGC, Mumbai, India.

On Friday, 31-08-2012 at 6.15 pm

At

Avion Hotel,

Domestic Airport, Nehru Road, Vile Parle (East), Mumbai - 400 057, India.

Mumbai Branch Tel No : (022) 25772637

Tel: (022) 25772637

Refer attached file for more details.


Regards,

 

Prem Nautiyal

The Indian Institute Of Welding

Mumbai Branch

Cell: 9769316004

 


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

Re: [MW:15171] Problem about Positive material Identification(PMI)

Mr. Jubir
 
Whether PMI was done before PWHT or after PWHT?
 
If results are from before PWHT, then there is something wrong in fillter metal, might be wrong fillter used.
 
If PMI done after PWHT, then you can weld sample joints again, and do PMI before and after PWHT and analyse the results.
 
Alternatively, you can try with other PMI isntruments, even you can go for Lab chemical analysis of few joints to ascertain some conclusion.
 
Thanks
 
Murugesan

On Fri, Aug 31, 2012 at 12:19 AM, c sridhar <sridhar305@yahoo.com> wrote:
 
Mr. Jubir,
Noted the points mentioned by you.  If the filler materials were pre checked and found to be OK for its chemistry, then there can not be any reason for such a drastic change in  the post weld chemistry, i.e., from 9% to 4%.
The pre, inter pass, post heat or PWHT  temp. as mentioned by you are all within the stipulated range and can not be a reason either.

All the 800 joints can not go wrong at a time unless something happened drastically. Have a random check (date wise fabrication) again and find  if  the Cr. deficiency  is same with all the joints. It may give an insight and may lead  to a conclusion.
regards,
Sridhar.



From: mohamed jubair <kmd.jubair@gmail.com>
To: materials-welding@googlegroups.com
Sent: Thursday, 30 August 2012 1:49 PM
Subject: Re: [MW:15164] Problem about Positive material Identification(PMI)

Dear Mr. Sridhar

Thanks for your suggestion.

Please understand my point. The filler wire readings mentioned in the table(trailing mail) is not from the manufacture's test certificate but from Positive material identification(PMI). In PMI test two parent metals,filler wire showing positive values as T91 but weld metal only not conforming as T91.

We procured other two new batch filler wires from the same manufacturer,welded and checked. It shows positive material for all the four(two parent metal,weld metal,filler wire) as T91.

Regards
Jubair
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

Thursday, August 30, 2012

[MW:15170] Invitation to IIW Monthly Technical Lecture_31st Aug 2012 @ Mumbai, India






Dear All,

Indian Institute of Welding, Mumbai branch cordially invites you for a technical lecture on

"Welding Requirements for Offshore Oil & Gas Projects"

By Mr. Maruti Kumar, AEE(E) / Mr. D. Badole, CE(M) / Mr Pradeep N. Nair, CE(E) From :QA & Vendor Cell, Offshore Engineering Services, ONGC, Mumbai, India.

On Friday, 31-08-2012 at 6.15 pm

At

Avion Hotel,

Domestic Airport, Nehru Road, Vile Parle (East), Mumbai - 400 057, India.

Mumbai Branch Tel No : (022) 25772637

Tel: (022) 25772637

Refer attached file for more details.


Regards,

 

Prem Nautiyal
The Indian Institute Of Welding
Mumbai Branch
Cell: 9769316004
 



--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

Re: [MW:15169] Problem about Positive material Identification(PMI)

 
Mr. Jubir,
Noted the points mentioned by you.  If the filler materials were pre checked and found to be OK for its chemistry, then there can not be any reason for such a drastic change in  the post weld chemistry, i.e., from 9% to 4%.
The pre, inter pass, post heat or PWHT  temp. as mentioned by you are all within the stipulated range and can not be a reason either.

All the 800 joints can not go wrong at a time unless something happened drastically. Have a random check (date wise fabrication) again and find  if  the Cr. deficiency  is same with all the joints. It may give an insight and may lead  to a conclusion.
regards,
Sridhar.



From: mohamed jubair <kmd.jubair@gmail.com>
To: materials-welding@googlegroups.com
Sent: Thursday, 30 August 2012 1:49 PM
Subject: Re: [MW:15164] Problem about Positive material Identification(PMI)

Dear Mr. Sridhar

Thanks for your suggestion.

Please understand my point. The filler wire readings mentioned in the table(trailing mail) is not from the manufacture's test certificate but from Positive material identification(PMI). In PMI test two parent metals,filler wire showing positive values as T91 but weld metal only not conforming as T91.

We procured other two new batch filler wires from the same manufacturer,welded and checked. It shows positive material for all the four(two parent metal,weld metal,filler wire) as T91.

Regards
Jubair
 

Re: [MW:15168] RE: 15142] Problem about Positive material Identification(PMI)

I request all our group members not to mention any consumable manufacturer's trade name in their queries.
This forum has to be STRICTLY used for exchange of technical information related to Welding, materials & NDT and not make a mockery of any company or do sales publicity across the globe for others. It takes years of hard work to earn reputation in the market and few seconds to lose the same. We are not here to cause harm to the reputation of any local Indian company and publicise international brands.
 
I hope you guys will cooperate and make the best use of this forum in a professional manner.
 
 
Regards
 
Prem Nautiyal
Cell: 9769316004
The Indian Institute Of Welding
Mumbai, India

--- On Wed, 8/29/12, Shankar gmail <shankarn6@gmail.com> wrote:

From: Shankar gmail <shankarn6@gmail.com>
Subject: Re: [MW:15151] RE: 15142] Problem about Positive material Identification(PMI)
To: materials-welding@googlegroups.com
Date: Wednesday, August 29, 2012, 8:42 AM

Dear Mr.Jubair,

 

I feel you have got 5Cr 1Mo wire from the supplier whereas they have produced 9Cr1Mo V  TC. it is not possible that the filler material chemistry and weld metal chemistry can change like this.

 

You have no other option but to cut and re-weld.  I would suggest that ban the supplier and be vigilant while procuring the consumables.

 

When you have trusted suppliers for this P91 alloy with long term reputation are in the market there is no need for you to venture with D&H. As such P91 is a critical alloy to deal with ( a lot of attention is required at every stage right from selection of consumables till proper PWHT) and the application is also critical any negligence on this could be disastrous.


regards,


shankar 






On Wed, Aug 29, 2012 at 4:48 AM, John Henning <jhenning@deltak.com> wrote:

You clearly have the wrong filler metal – you are out of spec for Cr, V, and Nb.  This filler metal will have far lower creep strength than the proper 91 chemistry filler metal.  You need to remove any weld found with this type chemistry and re-weld with proper filler metal.  If this filler metal is mismarked, you need to eliminate the supplier from your approved list.  This is a major problem and could have disastrous consequences if it makes it out into the field.

 

John A. Henning

Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of mohamed jubair
Sent: Tuesday, August 28, 2012 3:25 AM
To: materials-welding@googlegroups.com
Subject: [MW:15142] Problem about Positive material Identification(PMI)

 


Dear all,

 

In our  boiler one major problem occurred in Positive Material Identification(PMI) test [Spectrum test].  

 

Description

Reheater finishing outlet(RHFO) coil

Material

T91

Size

ø 63 x 4

Process

GTAW only

Filler wire

ER 90S B9

Filler wire Manufacturer

D & H Secheron

Preheating °C

185

Rate of Heating  °C

100/hr

Interpass temp  °C

190

Post heating  °C

100

PWHT  °C

750

Soaking Time

90 minutes

 

Around 800 joints welded in the above approved procedure only. Filler wire, header stub, RHFO coil, weld metal undergone PMI test separately and all show positive material results as T91 except weld metal. Weld metal shows the Chromium content only  as (4-7%){Reqd is 8-10.5%}.  We can't find how it happened? Our Chinese consultant told to cut and reweld all the joints. But our contractor argued that we followed approved procedure and used approved vendor's consumable only. Please give a solution. Here I have attached one preheating cum PWHT chart of RHFO joints(for 11 joints,5 thermocouples,1 recorder).All 800 joints are not checked yet. Only 40 joints checked and all 40 weld metals shown low Cr Content.

 

Please go through the below readings of one RHFO joint.

Description

Filler wire

Header stub

Weld metal

RHFO coil

 Alloy

T91

T91

A-2

T91

Cr

8.94

8.34

5.19

8.68

Mo

0.96

0.90

0.93

0.92

V

0.17

0.17

0.08

0.19

Ti

0.07

0.10

0.04

0.03

Mn

0.60

0.40

0.54

0.63

Fe

87.81

88.11

90.86

87.61

Ni

0.12

0.33

0.20

0.38

Cu

0.02

0.16

0.20

0.16

Nb

0.09

0.08

0.03

0.04

W

0.15

 

0.00

 

 

Waiting for your valuable suggestions.

 

Thanks & Regards

K Mohamed Jubair

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 
______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 



--
Shankar
9994562774
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

[MW:35738] ASME IX WPS Qualification Query: GTAW + FCAW with Multiple PQRs