Dear All,
In selection of the consumables please take note of the following points:
- Piling for Jetty is normally done by Hydraulic hammers
- Welding is carried out in situ and at horizontal position and SAW may not be possible( depending on the depth of Pile penetration)
- Immediately after the weld cools down it shall be subjected to RT and Piling continues to prevent the pile stuck in formation
- There will be no access to the root for back welding /grinding
- Root weld should be a full penetration
 
If the length of the Piles are known to be below 24 meters they may be welded in shop and the above points may not be applicable.
 
Regards
 
-----materials-welding@googlegroups.com wrote: -----

To: <materials-welding@googlegroups.com>
From: "pgoswami" <pgoswami@quickclic.net>
Sent by: materials-welding@googlegroups.com
Date: 01/30/2011 06:14PM
Subject: [MW:9561] Requirement of suitable welding consumables SAW and SMAW

Dear Muthu,
 
Here are some recommended consumables for X-65 steel, from Oerlikon and ESAB. The highlighted text would be of interest. For SAW along with OP-121TT flux oerlikons' recommendation is with 2 types of welding fillers(see the attachment).
 
If there are  NACE sour service requirements than MAX Nickel content should be 1%.
 
I would try to look for suitable wire flux combination from ESAB and get back to you.
 
You may call the representatives' of ESAB and Oerlikon, in case you need any assistance.
 
Thanks.
 
 
Pradip Goswami,P.Eng.IWE
Welding & Metallurgical Specialist & Consultant
Ontario, Canada.
Email-pgoswami@sympatico.ca,
 
 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of muthu barathi
Sent: Saturday, January 29, 2011 2:32 AM
To: materials-welding@googlegroups.com
Cc: pgoswami@sympatico.ca; pgoswami@quickclic.net
Subject: Re: RE: [MW:9546] Requirement of suitable welding consumables SAW and SMAW

Dear Sir

Actually this material is for Piling work. We are constructing a new    jetty . Steel Pile material is API - 5 L PSL - 2 / Grade X-65 . Pile
size OD - 1219mm and wall thickness - 22.22mm and also other size OD -    914mm and wall thickness - 22.22mm.

Now I want make a WPS by carrying out PQR . So I am searching based on    the sample pipe's MTC. The reading I have given is replica of MTC and
the is certified by Lloyds Surveyor too.

Now please tell me the correct welding electrode for SMAW and wire and    flux for SAW process. As per API 5L PSL 2 / Grade 65. the requirement -

X 65 - YS - 448 MPa. TS - 531 MPa. EL% - 23 - Impact at 0 deg.C 27 Joules. C - 0.22 Mn - 1.45 P- 0.025   S- 0.015 Ti - 0.06


Approved brands electrodes - ESAB and OERLIKON from these consumables   shall be selected.

While testing PQR it should not fail.

Expecting your mail shortly.

Thanking You.

With Regards,

Muthu Barathi P


On Fri, 28 Jan 2011 03:28:26 +0530 wrote
>


@font-face {
font-family: Tahoma;
}
@font-face {
font-family: Verdana;
}
@page Section1 {size: 595.45pt 841.7pt; margin: .1in .6in 0in .5in; }
P.MsoNormal {
MARGIN: 0in 0in 0pt; FONT-FAMILY: "Times New Roman"; FONT-SIZE:
12pt
}
LI.MsoNormal {
MARGIN: 0in 0in 0pt; FONT-FAMILY: "Times New Roman"; FONT-SIZE:
12pt
}
DIV.MsoNormal {
MARGIN: 0in 0in 0pt; FONT-FAMILY: "Times New Roman"; FONT-SIZE:
12pt
}
A:link {
COLOR: blue; TEXT-DECORATION: underline
}
SPAN.MsoHyperlink {
COLOR: blue; TEXT-DECORATION: underline
}
A:visited {
COLOR: blue; TEXT-DECORATION: underline
}
SPAN.MsoHyperlinkFollowed {
COLOR: blue; TEXT-DECORATION: underline
}
P {
FONT-FAMILY: "Times New Roman"; MARGIN-LEFT: 0in; FONT-SIZE:
12pt; MARGIN-RIGHT: 0in; mso-margin-top-alt: auto; mso-margin-bottom-
alt: auto
}
SPAN.EmailStyle18 {
FONT-FAMILY: Arial; COLOR: navy; mso-style-type: personal-reply
}
DIV.Section1 {
page: Section1
}



Mr. Muthu,

What's the applicable specification for this material,
ASTM/ASME/EN or any proprietary grade for any client or any vendor's
specification.The elongation and impact properties asked are highly
un-realistic. You never get a Carbon or Low Alloy steel with 46%
elongation
requirement, also, impact requirement is extremely high.

I would say, if you have any design paper work, which
indicates the grade or heat treatment of this steel the correct AWS
type of
welding consumables, SAW wire+flux specification etc could be worked
out.
Otherwise YOU SHOULD NEVER CHOOSE WELDING CONSUMABLES BASED ON THE
CHEMICAL
COMPOSITION ALONE.

Thanks.


Pradip Goswami,P.Eng.IWE
Welding & Metallurgical Specialist
& Consultant
Ontario, Canada.
Email-pgoswami@sympatico.ca,
pgoswami@quickclic.net

>


From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Pablo J
Acelajado
>Sent: Thursday, January 27, 2011 10:08 AM
>To:
materials-welding@googlegroups.com
>Subject: RE: [MW:9529] Requirement
of suitable welding consumables SAW and SMAW
>
>




January 27,
2011

Hello there!

This material is very strong one. I think
the welding consumable suppliers can best answer this question.

My understanding is that the percentage
elongationis not required for the weld.
Thank you.

Best regards.
PJA




From:
materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Kathalingam
Babu
>Sent: Thursday, January 27, 2011 1:10
PM
>To: materials-welding@googlegroups.com
>Subject: Re: [MW:9526] Requirement of
suitable welding consumables SAW and SMAW


Hi



The elongation requirement is very stringent, it is very
difficult to meet 46%, you have consult with the specific consumable
suppliers
to get 46%



Thanks & Regards,



K. Babu


>----- Original Message -----



From: muthu barathi


To: materials-welding@googlegroups.com


Sent: Thursday,
January 27, 2011 4:36 PM

Subject: [MW:9523]
Requirement of suitable welding consumables SAW and
SMAW


Hi Friends,
>
>Let me get your expertise of
selection of welding consumables in this
>regard.
>
>The base material
Chemical properties as given under (%):
>
>C - 0.066
>Si - 0.26
>Mn -
1.55
>P - 0.014
>S - 0.004
>Al - 0.046
>Cr - 0.186
>Ni - 0.015
>Mo
- 0.002
>Cu - 0.020
>V - 0.057
>Nb - 0.065
>Ti - 0.020
>N -
0.007
>B - 0.00025
>Ca - 0.0025
>CE - 0.371
>
>MECHANICAL
PROPERTIES
>YIELD STRENGTH - 516 MPa
>TENSILE STRENGTH - 625
MPa.
>ELONG % - 46
>IMOPACT
- (-) 10 DEGREE C - 250 JOULES
>
>NOW PLEASE TELL ME, WHICH
ELECTRODE FOR SMAW (BRAMDS ESAB, OERLIKON)
>AND SAW - FLUX AND WIRE WILL
SUIT AND PASS PQR TEST FOR PREPARATION OF
>WPS?
>
>PLEASE
HELP.
>THANKING YOU.
>
>
>
>Dear
Sir,
>
>
>
>
>
>Thanking You,
>
>Honesty is the best
Policy
>
>With Warm Regards,
>
>Muthu Barathi P
>Mobile
No:00962788269821 (Jordan)
>00962775401951





--
>To post to this group, send email to
materials-welding@googlegroups.com
>To
unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
>For more options, visit this
group's bolg at http://materials-welding.blogspot.com/
>The
views expressed/exchnaged in this group are members personel views
and meant
for educational purposes only, Users must take their own decisions
w.r.t.
applicable code/standard/contract
documents.
--
>To post to this group, send email to
materials-welding@googlegroups.com
>To unsubscribe from this group, send email
to materials-welding+unsubscribe@googlegroups.com
>For more options, visit
this group's bolg at http://materials-welding.blogspot.com/
>The
views expressed/exchnaged in this group are members personel views and
meant for
educational purposes only, Users must take their own decisions w.r.t.
applicable
code/standard/contract documents.
>
--
>To post to this group, send email to
materials-welding@googlegroups.com
>To unsubscribe from this group, send email
to materials-welding+unsubscribe@googlegroups.com
>For more options, visit
this group's bolg at http://materials-welding.blogspot.com/
>The
views expressed/exchnaged in this group are members personel views and
meant for
educational purposes only, Users must take their own decisions w.r.t.
applicable
code/standard/contract documents.
>



--
>
To post to this group, send email to materials-welding@googlegroups.com
>
To unsubscribe from this group, send email to materials-
welding+unsubscribe@googlegroups.com
>
For more options, visit this group's bolg at http://materials-
welding.blogspot.com/
>
The views expressed/exchnaged in this group are members personel views
and meant for educational purposes only, Users must take their own
decisions w.r.t. applicable code/standard/contract documents.
>


Dear Sir,





Thanking You,

Honesty is the best Policy

With Warm Regards,

Muthu Barathi P
Mobile No:00962788269821 (Jordan)
00962775401951

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



[attachment "OK 73.08.pdf" removed by Fred Majdnia/TECHNIP-ITALY]
[attachment "OP-121TT.pdf" removed by Fred Majdnia/TECHNIP-ITALY]
[attachment "TENAX 56ST-E 8018-G.pdf" removed by Fred Majdnia/TECHNIP-ITALY]
    This email and any attached files ("Message") may contain confidential and/or privileged information. It is intended solely for the addressee(s). If you receive this Message in error, inform the sender by reply email, delete the Message and destroy any printed copy. Any unauthorized use, distribution, or copying of this Message or any part thereof is prohibited. Emails are susceptible to alteration. Neither Technip nor any of its affiliates shall be liable for the Message if altered or falsified nor shall they be liable for any damage caused by any virus that might be transmitted with this Message. 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35738] ASME IX WPS Qualification Query: GTAW + FCAW with Multiple PQRs

Dear Welding Experts, I'm currently preparing a Welding Procedure Specification (WPS) and have encountered a request to qualify a GTAW +...