Hi
Pl. browse the reply already given in earlier thread - MW:4205 :
It's true that boiler or pressure vessel codes or structural welding codes do not specify the shelf-life or expiry dates of welding electrodes.
For example, ASME Nuclear Codes Sec-III, Clause & NB, NC-2440 specifies that:- Suitable storage and handling of electrodes, flux, and other welding materials shall be maintained. Precautions shall be taken to minimize absorption of moisture by fluxes and cored, fabricated, and coated electrodes.
The shelf-life of welding electrodes to a great extent depends on electrode manufacturer's methods, quality control procedure and how electrodes are handled. Depending on the coating type, packing (hermetically sealed or not), storing methods and ambient conditions, humidity etc, electrodes may last long or less. However as a good practice and based on electrode manufacturer's guidelines it may be worth considering:-
Ā· Solid Wires, GTAW/GMAW-No shelf Life.
Ā· Cored Wire āFCAW- No shelf life
Ā· SMAW ā The rule should be FIFO (First in First Out). Electrodes where the coating shows sign of flaking, cracks etc certainly should be discarded without much thoughts. Electrodes not older than 2-3 years but in good condition may be used. If required the diffusible hydrogen test could be repeated. Electrodes older than 3 years generally should not be used as a good engineering rule.
Ā· SAW Fluxes- Shelf life 2-3 years maximum subject to the flux condition and amount of fine particles/dust generated and behavior during welding.
Thanks.
Pradip Goswami, P.Eng
Regards
Prem Nautiyal
On Mon, 31 Jan 2011 09:48:41 +0530 wrote
>Dear Experts,
generally what is expiry period for SMAw consumables (Flux coated) dose ASME Sec II-C refers regarding this, if so please refer which class.in the consumable wraper only manufactured date is given but not the expiry date.
Thanks & Regards,
K.Pandiarajan.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
PREM S NAUTIYAL
CELL : 9769316004
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Pl. browse the reply already given in earlier thread - MW:4205 :
It's true that boiler or pressure vessel codes or structural welding codes do not specify the shelf-life or expiry dates of welding electrodes.
For example, ASME Nuclear Codes Sec-III, Clause & NB, NC-2440 specifies that:- Suitable storage and handling of electrodes, flux, and other welding materials shall be maintained. Precautions shall be taken to minimize absorption of moisture by fluxes and cored, fabricated, and coated electrodes.
The shelf-life of welding electrodes to a great extent depends on electrode manufacturer's methods, quality control procedure and how electrodes are handled. Depending on the coating type, packing (hermetically sealed or not), storing methods and ambient conditions, humidity etc, electrodes may last long or less. However as a good practice and based on electrode manufacturer's guidelines it may be worth considering:-
Ā· Solid Wires, GTAW/GMAW-No shelf Life.
Ā· Cored Wire āFCAW- No shelf life
Ā· SMAW ā The rule should be FIFO (First in First Out). Electrodes where the coating shows sign of flaking, cracks etc certainly should be discarded without much thoughts. Electrodes not older than 2-3 years but in good condition may be used. If required the diffusible hydrogen test could be repeated. Electrodes older than 3 years generally should not be used as a good engineering rule.
Ā· SAW Fluxes- Shelf life 2-3 years maximum subject to the flux condition and amount of fine particles/dust generated and behavior during welding.
Thanks.
Pradip Goswami, P.Eng
Regards
Prem Nautiyal
On Mon, 31 Jan 2011 09:48:41 +0530 wrote
>Dear Experts,
generally what is expiry period for SMAw consumables (Flux coated) dose ASME Sec II-C refers regarding this, if so please refer which class.in the consumable wraper only manufactured date is given but not the expiry date.
Thanks & Regards,
K.Pandiarajan.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
PREM S NAUTIYAL
CELL : 9769316004
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Comments