Sunday, October 31, 2021

Re: [MW:32589] SA 516 GR 70- AVOIDANCE OF PWHT - 40 mm thickness

Refer attached interpretations

On Sun, 31 Oct 2021, 10:30 Vishwas Keskar, <vvkeskar123@gmail.com> wrote:
Thanks for Sir.
Pl help for ref for Code or Code case.

On Fri, 29 Oct 2021, 21:40 pgoswami, <pgoswami@rogers.com> wrote:
Sec VIII,Div1:-
40 mm thickness calls for PWHT irrespective of service,  lethal or Non- Lethal. 
Would like to see in  DIV1,which code clause or code case,  allows application of buttering on C.S, PWHT of individual sections, welding of the closing seam by austenitic filler metal with no PWHT.

Thanks. 
P.Goswami. 




Sent from my Bell Samsung device over Canada's largest network.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/617c1ce1.1c69fb81.e31de.34e7SMTPIN_ADDED_MISSING%40gmr-mx.google.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADder3N4t9gCO%2B_BeK9hm%2Bh8G-U1tcHrxSHzqOyrmLiOqwxLFA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAEi5r3ZiHHg2VaOd_y6wKpiMpV3aY%3DoutaZPH2DB6rhQ2zB0%2BQ%40mail.gmail.com.

Re: [MW:32588] SA 516 GR 70- AVOIDANCE OF PWHT - 40 mm thickness

Dear Prasad 
Thanks for technical support.
Pl share where this was deployed.
Our vessel is ASME SEX VIII DIV 1 vessel
U stamping and TPI is involved.
Any Code back up , Code case  will be further helpful .

On Sun, 31 Oct 2021, 10:30 Prasad Ghanekar, <prsgne@gmail.com> wrote:
Sir,
1. In this case buttering is carried out prior to PWHT
2. PWHT is due to thickness of P1 material
3. No welding involved with P1 material in closing joint
4. PWHT is not mandatory for P8 welds.

That's my analysis and understanding.
We have implemented such practice in past due to some construction constraints.

Regards,
Prasad G.


On Fri, 29 Oct 2021, 21:40 pgoswami, <pgoswami@rogers.com> wrote:
Sec VIII,Div1:-
40 mm thickness calls for PWHT irrespective of service,  lethal or Non- Lethal. 
Would like to see in  DIV1,which code clause or code case,  allows application of buttering on C.S, PWHT of individual sections, welding of the closing seam by austenitic filler metal with no PWHT.

Thanks. 
P.Goswami. 




Sent from my Bell Samsung device over Canada's largest network.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/617c1ce1.1c69fb81.e31de.34e7SMTPIN_ADDED_MISSING%40gmr-mx.google.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAEi5r3b9ENgcV8DhsRJg2S%2B82%2B3FsVtHRndeQbV5VxunJKcNRw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADder3P_JS_krsoJuCXtY9fG%2B-G3nAQKQih0MU3wrX6NiZCSCw%40mail.gmail.com.

Saturday, October 30, 2021

Re: [MW:32580] SA 516 GR 70- AVOIDANCE OF PWHT - 40 mm thickness

Thanks for Sir.
Pl help for ref for Code or Code case.

On Fri, 29 Oct 2021, 21:40 pgoswami, <pgoswami@rogers.com> wrote:
Sec VIII,Div1:-
40 mm thickness calls for PWHT irrespective of service,  lethal or Non- Lethal. 
Would like to see in  DIV1,which code clause or code case,  allows application of buttering on C.S, PWHT of individual sections, welding of the closing seam by austenitic filler metal with no PWHT.

Thanks. 
P.Goswami. 




Sent from my Bell Samsung device over Canada's largest network.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/617c1ce1.1c69fb81.e31de.34e7SMTPIN_ADDED_MISSING%40gmr-mx.google.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADder3N4t9gCO%2B_BeK9hm%2Bh8G-U1tcHrxSHzqOyrmLiOqwxLFA%40mail.gmail.com.

Friday, October 29, 2021

Re: [MW:32579] SA 516 GR 70- AVOIDANCE OF PWHT - 40 mm thickness

X-Google-Smtp-Source: ABdhPJyXXqALmtSsmIcDmTC7sE2HBFMsLiFrEO1Apwq8hdP0dP2ClEj+dRZEPPQEferT/ybvqcFp
X-Received: by 2002:ad4:5747:: with SMTP id q7mr4731645qvx.19.1635523253612;
Fri, 29 Oct 2021 09:00:53 -0700 (PDT)
ARC-Seal: i=1; a=rsa-sha256; t=1635523253; cv=none;
d=google.com; s=arc-20160816;
b=Pa1emM+ao9FLI2YyzU5ueanl6w5EUr7ihwu0hwfwXxdY2iUAcNar/VwQgKyREyqq5l
iCUUBd9NC4hR51TlNYyMBgz5mNcHq8+XCtbySPndOu/d2xQl8702SkogyKfLGmmrqAuD
rZHr/OuS52uE2iYZ/vb3CtMzL/ljFNsmDPylh9pWFAN1FuERq84eccaBFYCVPCia3wLA
uDF5aM5opHuqHtT1MWSyF/7mbBRIDind0gS/1yxd/M2oeAPyC8caQiSeiQjPoW5wgWzx
7Moz1JFmM4svQD/TrLVP0F8yxGiT4syN0FNrQpyAVgTyEqTkh8AkMYRVBBg6io2or3Bi
bu2w==
ARC-Message-Signature: i=1; a=rsa-sha256; c=relaxed/relaxed; d=google.com; s=arc-20160816;
h=to:subject:message-id:date:from:in-reply-to:references:mime-version
:dkim-signature;
bh=Vp+cQqHJZpQ7LeNxLC3pIaMYBSTc4310IAIRi4NUDWk=;
b=S4Gp/PRLHAJnvY6kWjT+IycmjsqF9+PsE39Hi5OIxPoJgv8frjBMwdCg9hRVLu9uyB
AO2mQtyl9blZ0i9VedGIIoPBbbj7OOrux0g4MYNVGpj+OhVYbXWcOODytenEURiSJlz7
7/nyBL5WIWBdQPXnVb8WtBOLudiCi+SiTiyBWPXxoB9N+GoJUOUkV0cgiO9POOWSqxpw
KcHdwBqPnCQBBaKn956hjnxr8GRExTIlkdKsBwrfejqTbk14o01wIF+U3HNU8gJfjbpr
lrcLGIHHkXWFnvXMORNcCeFh566z9gDchWFI5AcXVItIQJVC5G7NaCXRGIkUPD71v6qW
upZQ==
ARC-Authentication-Results: i=1; gmr-mx.google.com;
dkim=pass header.i=@gmail.com header.s=20210112 header.b=L3EMTtQG;
spf=pass (google.com: domain of prsgne@gmail.com designates 2607:f8b0:4864:20::332 as permitted sender) smtp.mailfrom=prsgne@gmail.com;
dmarc=pass (p=NONE sp=QUARANTINE dis=NONE) header.from=gmail.com
Return-Path: <prsgne@gmail.com>
Received: from mail-ot1-x332.google.com (mail-ot1-x332.google.com. [2607:f8b0:4864:20::332])
by gmr-mx.google.com with ESMTPS id d9si256974qkn.7.2021.10.29.09.00.53
for <materials-welding@googlegroups.com>
(version=TLS1_3 cipher=TLS_AES_128_GCM_SHA256 bits=128/128);
Fri, 29 Oct 2021 09:00:53 -0700 (PDT)
Received-SPF: pass (google.com: domain of prsgne@gmail.com designates 2607:f8b0:4864:20::332 as permitted sender) client-ip=2607:f8b0:4864:20::332;
Authentication-Results: gmr-mx.google.com;
dkim=pass header.i=@gmail.com header.s=20210112 header.b=L3EMTtQG;
spf=pass (google.com: domain of prsgne@gmail.com designates 2607:f8b0:4864:20::332 as permitted sender) smtp.mailfrom=prsgne@gmail.com;
dmarc=pass (p=NONE sp=QUARANTINE dis=NONE) header.from=gmail.com
Received: by mail-ot1-x332.google.com with SMTP id v40-20020a056830092800b0055591caa9c6so5931896ott.4
for <materials-welding@googlegroups.com>; Fri, 29 Oct 2021 09:00:53 -0700 (PDT)
DKIM-Signature: v=1; a=rsa-sha256; c=relaxed/relaxed;
d=gmail.com; s=20210112;
h=mime-version:references:in-reply-to:from:date:message-id:subject:to;
bh=Vp+cQqHJZpQ7LeNxLC3pIaMYBSTc4310IAIRi4NUDWk=;
b=L3EMTtQGMSlcGeJSrsYgcL/fjHaHQQcVTNAl62EO/6C5URBhViNK6pNazNjX9b+39M
dPTmSYIzzpYDfxrX+u3rKjMk39875aCj0dDRwwS3wEX8RR+Da3dSCYWWdkAz6JY+qWq5
LCZ+92YSu/v/6+TU9525znNFM0LjCYXZ3PHjVGjF7eLVDz4RMMJGXSK0DnPSjef4Nm0L
Vo6A1f/9q7jDAzoYupXjYSjD5oQPns8y1rMU7HfTu3XJv2VDh3DwDBKu5V9obHNgfGCj
LoKMarFauYcW3Cik+h5MIpM16t1Ce7EW7KUTAwTxGwf+b7kc3AhgWN7LKYRhiOrt/cVH
Q/Nw==
X-Google-DKIM-Signature: v=1; a=rsa-sha256; c=relaxed/relaxed;
d=1e100.net; s=20210112;
h=x-gm-message-state:mime-version:references:in-reply-to:from:date
:message-id:subject:to;
bh=Vp+cQqHJZpQ7LeNxLC3pIaMYBSTc4310IAIRi4NUDWk=;
b=PNQTtqfpyaTNcHVfKZrKIYU7W6hjh7evWx0AcD5gARRse1eNrqwqfE7bNutfOCAgc9
sIup74mD51KP3J8AKhM7QiVbsF28zyzdBDatMwv2Q9JG6BO1fPGkVG63wFdq2T0Q0YQS
EWGsGyBIhY3TgQ8UhxuH2HhfEUQRd9Mjha16AEaOcXK9hWLvVmOH650HnjGtjkhz9Lzx
wX2tSt9tYfDQQ35CtLk9xp/9v2F1oJPGNPTOLFCKLFWuf4HDluvKFzNWcrpsvAZPlcWn
duwaa+mkyF4zJ4AdHyLeJorNjvE4vhWY8UFtBfKQf+f4GWC9ZKokgim1CAp5bh1CtxCn
dE/A==
X-Gm-Message-State: AOAM530IEU7A9MmNeb7kWqp6E6sI7g8qeNO3PQ9yrRVDrEMWOrvDdqsc
lJQovYfebKPzYU0PUQnOQf4iBkP5V3Zxc6ZVc6qnHH8K
X-Received: by 2002:a05:6830:1e95:: with SMTP id n21mr9064876otr.141.1635523252987;
Fri, 29 Oct 2021 09:00:52 -0700 (PDT)
MIME-Version: 1.0
References: <bdca7c90-9d2b-4df4-a685-5e7745a76351n@googlegroups.com>
<1026225126.1426146.1635504382367@mail.yahoo.com> <!&!AAAAAAAAAAAuAAAAAAAAABVPzeizzeRJsiPziIE5jXQBAMO2jhD3dRHOtM0AqgC7tuYAAAAAAA4AABAAAABjCD5+CS8gRrhVzbK+6VyIAQAAAAA=@rogers.com>
In-Reply-To: <!&!AAAAAAAAAAAuAAAAAAAAABVPzeizzeRJsiPziIE5jXQBAMO2jhD3dRHOtM0AqgC7tuYAAAAAAA4AABAAAABjCD5+CS8gRrhVzbK+6VyIAQAAAAA=@rogers.com>
From: Prasad Ghanekar <prsgne@gmail.com>
Date: Fri, 29 Oct 2021 21:30:40 +0530
Message-ID: <CAEi5r3a97dkQ4+qi3pbePCO7bxM_jB_P9K+r5-j0nHg9UJsDsg@mail.gmail.com>
Subject: Re: [MW:32578] SA 516 GR 70- AVOIDANCE OF PWHT - 40 mm thickness
To: materials-welding@googlegroups.com
Content-Type: multipart/alternative; boundary="0000000000008428a205cf7fee0a"

--0000000000008428a205cf7fee0a
Content-Type: text/plain; charset="UTF-8"
Content-Transfer-Encoding: quoted-printable

In my opinion As per ASME code, acceptable, no PWHT required for given
condition if welded with austenitic stainless Steel consumables.
However check service condition for dissimilar metal exposure to service
fluid and environment.

Regards,
Prasad G.

On Fri, 29 Oct 2021, 18:03 , <pgoswami@rogers.com> wrote:

> Hi Vishwas,
>
> Your query does not indicate the thickness , which is most critical aspec=
t
> of choosing the PWHT cycle.
>
> Irrespective of that, it=E2=80=99s not advisable to leave one joint, *esp=
ecially
> the closing joint* without PWHT and commission the vessel in service. You
> may better perform a LOCAL PWHT at the site.
>
> Also using dissimilar consumable is encouraged , only if dissimilar metal
> welding is involved. In this case use of dissimilar welding consumable is
> not desired, that may add undue thermal stress in service on the joint
> welded.
>
>
>
> Thanks.
>
>
>
> Pradip Goswami.P.Eng, IWE.
>
> Cell/Whasapp:1-905-9793232
>
>
>
> *From:* james gerald <gerry_tup@yahoo.com>
> *Sent:* October 29, 2021 6:46 AM
> *To:* materials-welding@googlegroups.com
> *Subject:* Re: [MW:32577] SA 516 GR 70- AVOIDANCE OF PWHT - 40 mm
> thickness
>
>
>
> Please experts to share on Designer's view with respect to different
> lateral expansion though Design temperature is +250degC
>
>
>
> *Thanks & Regards*
>
> *J.Gerald Jayakumar*
>
>
>
>
>
>
>
> On Friday, 29 October, 2021, 11:53:02 am GMT+4, Vishwas Keskar Welding
> Manager WELDING <vvkeskar123@gmail.com> wrote:
>
>
>
>
>
> The vessel details are
>
> MOC - SA 516 GR 70
>
> DIAMETER- 4020mm
>
> LENGTH - 37 MTR
>
> MDMT =3D - 50 Deg C to + 250 Deg C
>
> SERVICE - Non lethal /No Hydrogen Service
>
>
>
> We are proposing Vessel length build up as per FURNACE LENGTH CAPACITY(24
> m maximum) and one joint WITHOUT PWHT ( JOINING PWHTed sections earlier =
at
> site )
>
> Proposal -
>
> 1.MOC - SA 516 GR 70
>
> 2.BUTTERING - ENiCrFe2 on 24 m section end and other at 13 m section end)
>
> 3,PWHT (section PWHT - One of 24 length and other 13 m)
> of - 620 Deg C - 125 MINUTES
>
> 4.Bevel preparation
>
> 5.NDT - DPT
>
> Welding at site ( 24 m section with 13 m section) - ENiCrFe2 OR E309
>
> 6.NDT - DPT AND UT
>
>
>
> Expert opinion please and share experience if any
>
>
>
> Vishwas
>
>
>
> --
> https://materials-welding.blogspot.com/
> https://www.linkedin.com/groups/122787
> ---
> You received this message because you are subscribed to the Google Groups
> "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an
> email to materials-welding+unsubscribe@googlegroups.com.
> To view this discussion on the web visit
> https://groups.google.com/d/msgid/materials-welding/bdca7c90-9d2b-4df4-a6=
85-5e7745a76351n%40googlegroups.com

> <https://groups.google.com/d/msgid/materials-welding/bdca7c90-9d2b-4df4-a=
685-5e7745a76351n%40googlegroups.com?utm_medium=3Demail&utm_source=3Dfooter=

>
> .
>
>
> <http://www.avg.com/email-signature?utm_medium=3Demail&utm_source=3Dlink&=
utm_campaign=3Dsig-email&utm_content=3Demailclient
> Virus-free.
> www.avg.com
> <http://www.avg.com/email-signature?utm_medium=3Demail&utm_source=3Dlink&=
utm_campaign=3Dsig-email&utm_content=3Demailclient
>
> <#m_-9143628470932963806_DAB4FAD8-2DD7-40BB-A1B8-4E2AA1F9FDF2>
>
> --
> https://materials-welding.blogspot.com/
> https://www.linkedin.com/groups/122787
> ---
> You received this message because you are subscribed to the Google Groups
> "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an
> email to materials-welding+unsubscribe@googlegroups.com.
> To view this discussion on the web visit
> https://groups.google.com/d/msgid/materials-welding/!%26!AAAAAAAAAAAuAAAA=
AAAAABVPzeizzeRJsiPziIE5jXQBAMO2jhD3dRHOtM0AqgC7tuYAAAAAAA4AABAAAABjCD5%2BC=
S8gRrhVzbK%2B6VyIAQAAAAA%3D%40rogers.com
> <https://groups.google.com/d/msgid/materials-welding/!%26!AAAAAAAAAAAuAAA=
AAAAAABVPzeizzeRJsiPziIE5jXQBAMO2jhD3dRHOtM0AqgC7tuYAAAAAAA4AABAAAABjCD5%2B=
CS8gRrhVzbK%2B6VyIAQAAAAA%3D%40rogers.com?utm_medium=3Demail&utm_source=3Df=
ooter>
> .
>

--0000000000008428a205cf7fee0a
Content-Type: text/html; charset="UTF-8"
Content-Transfer-Encoding: quoted-printable

<div dir=3D"auto">In my opinion As per ASME code, acceptable, no PWHT requi=
red for given condition if welded with austenitic stainless Steel consumabl=
es.<div dir=3D"auto">However check service condition for dissimilar metal e=
xposure to service fluid and environment.</div><div dir=3D"auto"><br></div>=
<div dir=3D"auto">Regards,</div><div dir=3D"auto">Prasad G.</div></div><br>=
<div class=3D"gmail_quote"><div dir=3D"ltr" class=3D"gmail_attr">On Fri, 29=
Oct 2021, 18:03 , &lt;<a href=3D"mailto:pgoswami@rogers.com">pgoswami@roge=
rs.com</a>&gt; wrote:<br></div><blockquote class=3D"gmail_quote" style=3D"m=
argin:0 0 0 .8ex;border-left:1px #ccc solid;padding-left:1ex"><div lang=3D"=
EN-US" link=3D"blue" vlink=3D"purple" style=3D"word-wrap:break-word"><div c=
lass=3D"m_-9143628470932963806WordSection1"><p class=3D"MsoNormal"><span st=
yle=3D"font-size:12.0pt">Hi Vishwas,<u></u><u></u></span></p><p class=3D"Ms=
oNormal"><span style=3D"font-size:12.0pt">Your query does not indicate the =
thickness , which is most critical aspect of choosing the PWHT cycle. <u></=
u><u></u></span></p><p class=3D"MsoNormal"><span style=3D"font-size:12.0pt"=
>Irrespective of that, it=E2=80=99s not advisable to leave one joint, <u>es=
pecially the closing joint</u> without PWHT and commission the vessel in se=
rvice. You may better perform a LOCAL PWHT at the site. <u></u><u></u></spa=
n></p><p class=3D"MsoNormal"><span style=3D"font-size:12.0pt">Also using di=
ssimilar consumable is encouraged , only if dissimilar metal welding is inv=
olved. In this case use of dissimilar welding consumable is not desired, th=
at may add undue thermal stress in service on the joint welded. <u></u><u><=
/u></span></p><p class=3D"MsoNormal"><span style=3D"font-size:12.0pt"><u></=
u>=C2=A0<u></u></span></p><p class=3D"MsoNormal"><span style=3D"font-size:1=
2.0pt">Thanks.<u></u><u></u></span></p><p class=3D"MsoNormal"><span style=
=3D"font-size:12.0pt"><u></u>=C2=A0<u></u></span></p><div><p class=3D"MsoNo=
rmal"><span lang=3D"EN-CA" style=3D"font-size:10.0pt;font-family:&quot;Taho=
ma&quot;,sans-serif">Pradip Goswami.P.Eng, IWE.<u></u><u></u></span></p><p =
class=3D"MsoNormal"><span lang=3D"EN-CA" style=3D"font-size:10.0pt;font-fam=
ily:&quot;Tahoma&quot;,sans-serif">Cell/Whasapp:1-905-9793232</span><span s=
tyle=3D"font-size:10.0pt;font-family:&quot;Tahoma&quot;,sans-serif"><u></u>=
<u></u></span></p></div><p class=3D"MsoNormal"><span style=3D"font-size:12.=
0pt"><u></u>=C2=A0<u></u></span></p><div><div style=3D"border:none;border-t=
op:solid #e1e1e1 1.0pt;padding:3.0pt 0cm 0cm 0cm"><p class=3D"MsoNormal"><b=
>From:</b> james gerald &lt;<a href=3D"mailto:gerry_tup@yahoo.com" target=
=3D"_blank" rel=3D"noreferrer">gerry_tup@yahoo.com</a>&gt; <br><b>Sent:</b>=
October 29, 2021 6:46 AM<br><b>To:</b> <a href=3D"mailto:materials-welding=
@googlegroups.com" target=3D"_blank" rel=3D"noreferrer">materials-welding@g=
ooglegroups.com</a><br><b>Subject:</b> Re: [MW:32577] SA 516 GR 70- AVOIDAN=
CE OF PWHT - 40 mm thickness<u></u><u></u></p></div></div><p class=3D"MsoNo=
rmal"><u></u>=C2=A0<u></u></p><div><div><div><p class=3D"MsoNormal"><span s=
tyle=3D"font-size:12.0pt;font-family:&quot;Helvetica&quot;,sans-serif">Plea=
se experts to share on Designer&#39;s view with respect to different latera=
l expansion though Design temperature is +250degC<u></u><u></u></span></p><=
/div><div><p class=3D"MsoNormal"><span style=3D"font-size:12.0pt;font-famil=
y:&quot;Helvetica&quot;,sans-serif"><u></u>=C2=A0<u></u></span></p></div><d=
iv><div><p><em><span style=3D"font-size:12.0pt;font-family:&quot;Helvetica&=
quot;,sans-serif;color:#652191">Thanks &amp; Regards</span></em><span style=
=3D"font-size:12.0pt;font-family:&quot;Helvetica&quot;,sans-serif"><u></u><=
u></u></span></p><p><strong><span style=3D"font-size:12.0pt;font-family:&qu=
ot;Helvetica&quot;,sans-serif">J.Gerald Jayakumar</span></strong><span styl=
e=3D"font-size:12.0pt;font-family:&quot;Helvetica&quot;,sans-serif"><u></u>=
<u></u></span></p><p><span style=3D"font-size:12.0pt;font-family:&quot;Helv=
etica&quot;,sans-serif"><u></u>=C2=A0<u></u></span></p></div></div></div><d=
iv><p class=3D"MsoNormal"><span style=3D"font-size:12.0pt;font-family:&quot=
;Helvetica&quot;,sans-serif"><u></u>=C2=A0<u></u></span></p></div><div><p c=
lass=3D"MsoNormal"><span style=3D"font-size:12.0pt;font-family:&quot;Helvet=
ica&quot;,sans-serif"><u></u>=C2=A0<u></u></span></p></div></div><div id=3D=
"m_-9143628470932963806ydp6ffa7bc0yahoo_quoted_5925255893"><div><div><p cla=
ss=3D"MsoNormal"><span style=3D"font-size:10.0pt;font-family:&quot;Helvetic=
a&quot;,sans-serif;color:#26282a">On Friday, 29 October, 2021, 11:53:02 am =
GMT+4, Vishwas Keskar Welding Manager WELDING &lt;<a href=3D"mailto:vvkeska=
r123@gmail.com" target=3D"_blank" rel=3D"noreferrer">vvkeskar123@gmail.com<=
/a>&gt; wrote: <u></u><u></u></span></p></div><div><p class=3D"MsoNormal"><=
span style=3D"font-size:10.0pt;font-family:&quot;Helvetica&quot;,sans-serif=
;color:#26282a"><u></u>=C2=A0<u></u></span></p></div><div><p class=3D"MsoNo=
rmal"><span style=3D"font-size:10.0pt;font-family:&quot;Helvetica&quot;,san=
s-serif;color:#26282a"><u></u>=C2=A0<u></u></span></p></div><div><div id=3D=
"m_-9143628470932963806ydp6ffa7bc0yiv3628008508"><p class=3D"MsoNormal"><sp=
an style=3D"font-size:10.0pt;font-family:&quot;Helvetica&quot;,sans-serif;c=
olor:#26282a">The vessel details are=C2=A0<u></u><u></u></span></p><div><p =
class=3D"MsoNormal"><span style=3D"font-size:10.0pt;font-family:&quot;Helve=
tica&quot;,sans-serif;color:#26282a">MOC - SA 516 GR 70=C2=A0<u></u><u></u>=
</span></p></div><div><p class=3D"MsoNormal"><span style=3D"font-size:10.0p=
t;font-family:&quot;Helvetica&quot;,sans-serif;color:#26282a">DIAMETER- 402=
0mm<u></u><u></u></span></p></div><div><p class=3D"MsoNormal"><span style=
=3D"font-size:10.0pt;font-family:&quot;Helvetica&quot;,sans-serif;color:#26=
282a">LENGTH - 37 MTR<u></u><u></u></span></p></div><div><p class=3D"MsoNor=
mal"><span style=3D"font-size:10.0pt;font-family:&quot;Helvetica&quot;,sans=
-serif;color:#26282a">MDMT =3D - 50 Deg C to=C2=A0 + 250 Deg C=C2=A0<u></u>=
<u></u></span></p></div><div><p class=3D"MsoNormal"><span style=3D"font-siz=
e:10.0pt;font-family:&quot;Helvetica&quot;,sans-serif;color:#26282a">SERVIC=
E - Non lethal /No Hydrogen Service=C2=A0<u></u><u></u></span></p></div><di=
v><p class=3D"MsoNormal"><span style=3D"font-size:10.0pt;font-family:&quot;=
Helvetica&quot;,sans-serif;color:#26282a"><u></u>=C2=A0<u></u></span></p></=
div><div><p class=3D"MsoNormal"><span style=3D"font-size:10.0pt;font-family=
:&quot;Helvetica&quot;,sans-serif;color:#26282a">We are proposing Vessel le=
ngth build up as per FURNACE LENGTH CAPACITY(24 m maximum) and one joint WI=
THOUT PWHT=C2=A0 ( JOINING PWHTed sections earlier at site )<u></u><u></u><=
/span></p></div><div><p class=3D"MsoNormal"><span style=3D"font-size:10.0pt=
;font-family:&quot;Helvetica&quot;,sans-serif;color:#26282a">Proposal -=C2=
=A0<u></u><u></u></span></p></div><div><p class=3D"MsoNormal"><span style=
=3D"font-size:10.0pt;font-family:&quot;Helvetica&quot;,sans-serif;color:#26=
282a">1.MOC - SA 516 GR 70=C2=A0<u></u><u></u></span></p></div><div><p clas=
s=3D"MsoNormal"><span style=3D"font-size:10.0pt;font-family:&quot;Helvetica=
&quot;,sans-serif;color:#26282a">2.BUTTERING - ENiCrFe2 on 24 m section end=
and other at 13 m section end)<u></u><u></u></span></p></div><div><p class=
=3D"MsoNormal"><span style=3D"font-size:10.0pt;font-family:&quot;Helvetica&=
quot;,sans-serif;color:#26282a">3,PWHT (section PWHT - One of 24=C2=A0 leng=
th and other 13 m)<br>=C2=A0of=C2=A0 - 620 Deg C - 125 MINUTES=C2=A0<u></u>=
<u></u></span></p></div><div><p class=3D"MsoNormal"><span style=3D"font-siz=
e:10.0pt;font-family:&quot;Helvetica&quot;,sans-serif;color:#26282a">4.Beve=
l preparation=C2=A0<u></u><u></u></span></p></div><div><p class=3D"MsoNorma=
l"><span style=3D"font-size:10.0pt;font-family:&quot;Helvetica&quot;,sans-s=
erif;color:#26282a">5.NDT - DPT=C2=A0<u></u><u></u></span></p></div><div><p=
class=3D"MsoNormal"><span style=3D"font-size:10.0pt;font-family:&quot;Helv=
etica&quot;,sans-serif;color:#26282a">Welding at site ( 24 m section with 1=
3 m section) - ENiCrFe2 OR E309=C2=A0<u></u><u></u></span></p></div><div><p=
class=3D"MsoNormal"><span style=3D"font-size:10.0pt;font-family:&quot;Helv=
etica&quot;,sans-serif;color:#26282a">6.NDT - DPT AND UT<u></u><u></u></spa=
n></p></div><div><p class=3D"MsoNormal"><span style=3D"font-size:10.0pt;fon=
t-family:&quot;Helvetica&quot;,sans-serif;color:#26282a"><u></u>=C2=A0<u></=
u></span></p></div><div><p class=3D"MsoNormal"><span style=3D"font-size:10.=
0pt;font-family:&quot;Helvetica&quot;,sans-serif;color:#26282a">Expert opin=
ion please=C2=A0 and share experience if any=C2=A0<u></u><u></u></span></p>=
</div><div><p class=3D"MsoNormal"><span style=3D"font-size:10.0pt;font-fami=
ly:&quot;Helvetica&quot;,sans-serif;color:#26282a"><u></u>=C2=A0<u></u></sp=
an></p></div><div><p class=3D"MsoNormal"><span style=3D"font-size:10.0pt;fo=
nt-family:&quot;Helvetica&quot;,sans-serif;color:#26282a">Vishwas=C2=A0<u><=
/u><u></u></span></p></div><div><p class=3D"MsoNormal"><span style=3D"font-=
size:10.0pt;font-family:&quot;Helvetica&quot;,sans-serif;color:#26282a"><u>=
</u>=C2=A0<u></u></span></p></div><p class=3D"MsoNormal"><span style=3D"fon=
t-size:10.0pt;font-family:&quot;Helvetica&quot;,sans-serif;color:#26282a">-=
- <br><a href=3D"https://materials-welding.blogspot.com/" target=3D"_blank"=
rel=3D"noreferrer">https://materials-welding.blogspot.com/</a><br><a href=
=3D"https://www.linkedin.com/groups/122787" target=3D"_blank" rel=3D"norefe=
rrer">https://www.linkedin.com/groups/122787</a><br>--- <br>You received th=
is message because you are subscribed to the Google Groups &quot;Materials =
&amp; Welding&quot; group.<br>To unsubscribe from this group and stop recei=
ving emails from it, send an email to <a href=3D"mailto:materials-welding+u=
nsubscribe@googlegroups.com" target=3D"_blank" rel=3D"noreferrer">materials=
-welding+unsubscribe@googlegroups.com</a>.<br>To view this discussion on th=
e web visit <a href=3D"https://groups.google.com/d/msgid/materials-welding/=
bdca7c90-9d2b-4df4-a685-5e7745a76351n%40googlegroups.com?utm_medium=3Demail=
&amp;utm_source=3Dfooter
" target=3D"_blank" rel=3D"noreferrer">https://grou=
ps.google.com/d/msgid/materials-welding/bdca7c90-9d2b-4df4-a685-5e7745a7635=
1n%40googlegroups.com
</a>.<u></u><u></u></span></p></div></div></div></div>=
</div><div id=3D"m_-9143628470932963806DAB4FAD8-2DD7-40BB-A1B8-4E2AA1F9FDF2=
"><br>
<table style=3D"border-top:1px solid #d3d4de">
<tr>
<td style=3D"width:55px;padding-top:13px"><a href=3D"http://www.avg=
.com/email-signature?utm_medium=3Demail&amp;utm_source=3Dlink&amp;utm_campa=
ign=3Dsig-email&amp;utm_content=3Demailclient" target=3D"_blank" rel=3D"nor=
eferrer"><img src=3D"https://ipmcdn.avast.com/images/icons/icon-envelope-ti=
ck-green-avg-v1.png
" alt=3D"" width=3D"46" height=3D"29" style=3D"width:46p=
x;height:29px"></a></td>
<td style=3D"width:470px;padding-top:12px;color:#41424e;font-size:13px;fo=
nt-family:Arial,Helvetica,sans-serif;line-height:18px">Virus-free. <a href=
=3D"http://www.avg.com/email-signature?utm_medium=3Demail&amp;utm_source=3D=
link&amp;utm_campaign=3Dsig-email&amp;utm_content=3Demailclient
" style=3D"c=
olor:#4453ea" target=3D"_blank" rel=3D"noreferrer">www.avg.com</a>
</td>
</tr>
</table><a href=3D"#m_-9143628470932963806_DAB4FAD8-2DD7-40BB-A1B8-4E2AA1F9=
FDF2" width=3D"1" height=3D"1" rel=3D"noreferrer"> </a></div></div>

<p></p>

-- <br>
<a href=3D"https://materials-welding.blogspot.com/" target=3D"_blank" rel=
=3D"noreferrer">https://materials-welding.blogspot.com/</a><br>
<a href=3D"https://www.linkedin.com/groups/122787" target=3D"_blank" rel=3D=
"noreferrer">https://www.linkedin.com/groups/122787</a><br>
--- <br>
You received this message because you are subscribed to the Google Groups &=
quot;Materials &amp; Welding&quot; group.<br>
To unsubscribe from this group and stop receiving emails from it, send an e=
mail to <a href=3D"mailto:materials-welding+unsubscribe@googlegroups.com" t=
arget=3D"_blank" rel=3D"noreferrer">materials-welding+unsubscribe@googlegro=
ups.com</a>.<br>
To view this discussion on the web visit <a href=3D"https://groups.google.c=
om/d/msgid/materials-welding/!%26!AAAAAAAAAAAuAAAAAAAAABVPzeizzeRJsiPziIE5j=
XQBAMO2jhD3dRHOtM0AqgC7tuYAAAAAAA4AABAAAABjCD5%2BCS8gRrhVzbK%2B6VyIAQAAAAA%=
3D%40rogers.com?utm_medium=3Demail&amp;utm_source=3Dfooter" target=3D"_blan=
k" rel=3D"noreferrer">https://groups.google.com/d/msgid/materials-welding/!=
%26!AAAAAAAAAAAuAAAAAAAAABVPzeizzeRJsiPziIE5jXQBAMO2jhD3dRHOtM0AqgC7tuYAAAA=
AAA4AABAAAABjCD5%2BCS8gRrhVzbK%2B6VyIAQAAAAA%3D%40rogers.com</a>.<br>
</blockquote></div>

--0000000000008428a205cf7fee0a--
Sec VIII,Div1:-
40 mm thickness calls for PWHT irrespective of service,  lethal or Non- Lethal. 
Would like to see in  DIV1,which code clause or code case,  allows application of buttering on C.S, PWHT of individual sections, welding of the closing seam by austenitic filler metal with no PWHT.

Thanks. 
P.Goswami. 




Sent from my Bell Samsung device over Canada's largest network.

materials-welding - Google Groups: Message Pending [{IJunsqurt-azUyoCcWswA8OHXqjVmP2-0}]

A message has been sent to the materials-welding group and is awaiting approval. We've included this message for your review.

The message requires moderation because the user does not have permission to post.

You can approve or reject this message or you can approve this message by replying to this email.

RE: [MW:32580] SA 516 GR 70- AVOIDANCE OF PWHT - 40 mm thickness

Dear Vishwas, 

If you want avoid the PWHT localized and  the impact test, review the engineering specification for this vessel, what is required, the qualified WPS, type of process and electrodes used. 

if you buttering with ENiCrFe2 and finish  with E-309, you are creating a dissimilar weld on the vessel. Does the qualified WPS authorize it? 

Regards, 

Ramon Briceño

www.linkedin.com/in/ramonbriceno-metalengineer







De: materials-welding@googlegroups.com <materials-welding@googlegroups.com> en nombre de Vishwas Keskar Welding Manager WELDING <vvkeskar123@gmail.com>
Enviado: viernes, 29 de octubre de 2021 3:47 a. m.
Para: Materials & Welding <materials-welding@googlegroups.com>
Asunto: [MW:32577] SA 516 GR 70- AVOIDANCE OF PWHT - 40 mm thickness
 
The vessel details are 
MOC - SA 516 GR 70 
DIAMETER- 4020mm
LENGTH - 37 MTR
MDMT = - 50 Deg C to  + 250 Deg C 
SERVICE - Non lethal /No Hydrogen Service 

We are proposing Vessel length build up as per FURNACE LENGTH CAPACITY(24 m maximum) and one joint WITHOUT PWHT  ( JOINING PWHTed sections earlier at site )
Proposal - 
1.MOC - SA 516 GR 70 
2.BUTTERING - ENiCrFe2 on 24 m section end and other at 13 m section end)
3,PWHT (section PWHT - One of 24  length and other 13 m)
 of  - 620 Deg C - 125 MINUTES 
4.Bevel preparation 
5.NDT - DPT 
Welding at site ( 24 m section with 13 m section) - ENiCrFe2 OR E309 
6.NDT - DPT AND UT

Expert opinion please  and share experience if any 

Vishwas 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/bdca7c90-9d2b-4df4-a685-5e7745a76351n%40googlegroups.com.

Re: [MW:32580] SA 516 GR 70- AVOIDANCE OF PWHT - 40 mm thickness

Since your furnace length is 24meters, you have the option to pWHT the entire vessel as provided in the code below with minimum overlap. First PWHT one end for 24meters and then PWHT the another end by reversing with required overlap

Inline image

Thanks & Regards

J.Gerald Jayakumar




On Friday, 29 October, 2021, 02:46:22 pm GMT+4, james gerald <gerry_tup@yahoo.com> wrote:


Please experts to share on Designer's view with respect to different lateral expansion though Design temperature is +250degC

Thanks & Regards

J.Gerald Jayakumar




On Friday, 29 October, 2021, 11:53:02 am GMT+4, Vishwas Keskar Welding Manager WELDING <vvkeskar123@gmail.com> wrote:


The vessel details are 
MOC - SA 516 GR 70 
DIAMETER- 4020mm
LENGTH - 37 MTR
MDMT = - 50 Deg C to  + 250 Deg C 
SERVICE - Non lethal /No Hydrogen Service 

We are proposing Vessel length build up as per FURNACE LENGTH CAPACITY(24 m maximum) and one joint WITHOUT PWHT  ( JOINING PWHTed sections earlier at site )
Proposal - 
1.MOC - SA 516 GR 70 
2.BUTTERING - ENiCrFe2 on 24 m section end and other at 13 m section end)
3,PWHT (section PWHT - One of 24  length and other 13 m)
 of  - 620 Deg C - 125 MINUTES 
4.Bevel preparation 
5.NDT - DPT 
Welding at site ( 24 m section with 13 m section) - ENiCrFe2 OR E309 
6.NDT - DPT AND UT

Expert opinion please  and share experience if any 

Vishwas 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/bdca7c90-9d2b-4df4-a685-5e7745a76351n%40googlegroups.com.

Re: [MW:32580] SA 516 GR 70- AVOIDANCE OF PWHT - 40 mm thickness

Sir ,

its 40 mm thickness shell.

On Fri, 29 Oct 2021, 18:03 , <pgoswami@rogers.com> wrote:

Hi Vishwas,

Your query does not indicate the thickness , which is most critical aspect of choosing the PWHT cycle.

Irrespective of that, it's not advisable to leave one joint, especially the closing joint without PWHT and commission the vessel in service. You may better perform a LOCAL PWHT at the site.

Also using dissimilar consumable is encouraged , only if dissimilar metal welding is involved. In this case use of dissimilar welding consumable is not desired, that may add undue thermal stress in service on the joint welded.

 

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Cell/Whasapp:1-905-9793232

 

From: james gerald <gerry_tup@yahoo.com>
Sent: October 29, 2021 6:46 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:32577] SA 516 GR 70- AVOIDANCE OF PWHT - 40 mm thickness

 

Please experts to share on Designer's view with respect to different lateral expansion though Design temperature is +250degC

 

Thanks & Regards

J.Gerald Jayakumar

 

 

 

On Friday, 29 October, 2021, 11:53:02 am GMT+4, Vishwas Keskar Welding Manager WELDING <vvkeskar123@gmail.com> wrote:

 

 

The vessel details are 

MOC - SA 516 GR 70 

DIAMETER- 4020mm

LENGTH - 37 MTR

MDMT = - 50 Deg C to  + 250 Deg C 

SERVICE - Non lethal /No Hydrogen Service 

 

We are proposing Vessel length build up as per FURNACE LENGTH CAPACITY(24 m maximum) and one joint WITHOUT PWHT  ( JOINING PWHTed sections earlier at site )

Proposal - 

1.MOC - SA 516 GR 70 

2.BUTTERING - ENiCrFe2 on 24 m section end and other at 13 m section end)

3,PWHT (section PWHT - One of 24  length and other 13 m)
 of  - 620 Deg C - 125 MINUTES 

4.Bevel preparation 

5.NDT - DPT 

Welding at site ( 24 m section with 13 m section) - ENiCrFe2 OR E309 

6.NDT - DPT AND UT

 

Expert opinion please  and share experience if any 

 

Vishwas 

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/bdca7c90-9d2b-4df4-a685-5e7745a76351n%40googlegroups.com.


Virus-free. www.avg.com

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/!%26!AAAAAAAAAAAuAAAAAAAAABVPzeizzeRJsiPziIE5jXQBAMO2jhD3dRHOtM0AqgC7tuYAAAAAAA4AABAAAABjCD5%2BCS8gRrhVzbK%2B6VyIAQAAAAA%3D%40rogers.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADder3MJeMcwm-q782fK_XP0%3Dt7R%2Bz5jY1vmUb%2BD4J%2BNywodGA%40mail.gmail.com.

RE: [MW:32578] SA 516 GR 70- AVOIDANCE OF PWHT - 40 mm thickness

Hi Vishwas,

Your query does not indicate the thickness , which is most critical aspect of choosing the PWHT cycle.

Irrespective of that, it's not advisable to leave one joint, especially the closing joint without PWHT and commission the vessel in service. You may better perform a LOCAL PWHT at the site.

Also using dissimilar consumable is encouraged , only if dissimilar metal welding is involved. In this case use of dissimilar welding consumable is not desired, that may add undue thermal stress in service on the joint welded.

 

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Cell/Whasapp:1-905-9793232

 

From: james gerald <gerry_tup@yahoo.com>
Sent: October 29, 2021 6:46 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:32577] SA 516 GR 70- AVOIDANCE OF PWHT - 40 mm thickness

 

Please experts to share on Designer's view with respect to different lateral expansion though Design temperature is +250degC

 

Thanks & Regards

J.Gerald Jayakumar

 

 

 

On Friday, 29 October, 2021, 11:53:02 am GMT+4, Vishwas Keskar Welding Manager WELDING <vvkeskar123@gmail.com> wrote:

 

 

The vessel details are 

MOC - SA 516 GR 70 

DIAMETER- 4020mm

LENGTH - 37 MTR

MDMT = - 50 Deg C to  + 250 Deg C 

SERVICE - Non lethal /No Hydrogen Service 

 

We are proposing Vessel length build up as per FURNACE LENGTH CAPACITY(24 m maximum) and one joint WITHOUT PWHT  ( JOINING PWHTed sections earlier at site )

Proposal - 

1.MOC - SA 516 GR 70 

2.BUTTERING - ENiCrFe2 on 24 m section end and other at 13 m section end)

3,PWHT (section PWHT - One of 24  length and other 13 m)
 of  - 620 Deg C - 125 MINUTES 

4.Bevel preparation 

5.NDT - DPT 

Welding at site ( 24 m section with 13 m section) - ENiCrFe2 OR E309 

6.NDT - DPT AND UT

 

Expert opinion please  and share experience if any 

 

Vishwas 

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/bdca7c90-9d2b-4df4-a685-5e7745a76351n%40googlegroups.com.


Virus-free. www.avg.com

Re: [MW:32580] SA 516 GR 70- AVOIDANCE OF PWHT - 40 mm thickness

Please experts to share on Designer's view with respect to different lateral expansion though Design temperature is +250degC

Thanks & Regards

J.Gerald Jayakumar




On Friday, 29 October, 2021, 11:53:02 am GMT+4, Vishwas Keskar Welding Manager WELDING <vvkeskar123@gmail.com> wrote:


The vessel details are 
MOC - SA 516 GR 70 
DIAMETER- 4020mm
LENGTH - 37 MTR
MDMT = - 50 Deg C to  + 250 Deg C 
SERVICE - Non lethal /No Hydrogen Service 

We are proposing Vessel length build up as per FURNACE LENGTH CAPACITY(24 m maximum) and one joint WITHOUT PWHT  ( JOINING PWHTed sections earlier at site )
Proposal - 
1.MOC - SA 516 GR 70 
2.BUTTERING - ENiCrFe2 on 24 m section end and other at 13 m section end)
3,PWHT (section PWHT - One of 24  length and other 13 m)
 of  - 620 Deg C - 125 MINUTES 
4.Bevel preparation 
5.NDT - DPT 
Welding at site ( 24 m section with 13 m section) - ENiCrFe2 OR E309 
6.NDT - DPT AND UT

Expert opinion please  and share experience if any 

Vishwas 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/bdca7c90-9d2b-4df4-a685-5e7745a76351n%40googlegroups.com.

Re: [MW:32580] SA 516 GR 70- AVOIDANCE OF PWHT - 40 mm thickness

Normally the use of Nickel electrodes to avoid PWHT was practised in the SR(self reinforced) Nozzles where the vessel is not PWHTed and the Nozzle weld requires PWHT. Experts can throw some light on the C seam and any code restrictions.

Thanks & Regards

J.Gerald Jayakumar



On Friday, 29 October, 2021, 11:53:02 am GMT+4, Vishwas Keskar Welding Manager WELDING <vvkeskar123@gmail.com> wrote:


The vessel details are 
MOC - SA 516 GR 70 
DIAMETER- 4020mm
LENGTH - 37 MTR
MDMT = - 50 Deg C to  + 250 Deg C 
SERVICE - Non lethal /No Hydrogen Service 

We are proposing Vessel length build up as per FURNACE LENGTH CAPACITY(24 m maximum) and one joint WITHOUT PWHT  ( JOINING PWHTed sections earlier at site )
Proposal - 
1.MOC - SA 516 GR 70 
2.BUTTERING - ENiCrFe2 on 24 m section end and other at 13 m section end)
3,PWHT (section PWHT - One of 24  length and other 13 m)
 of  - 620 Deg C - 125 MINUTES 
4.Bevel preparation 
5.NDT - DPT 
Welding at site ( 24 m section with 13 m section) - ENiCrFe2 OR E309 
6.NDT - DPT AND UT

Expert opinion please  and share experience if any 

Vishwas 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/bdca7c90-9d2b-4df4-a685-5e7745a76351n%40googlegroups.com.

[MW:32577] SA 516 GR 70- AVOIDANCE OF PWHT - 40 mm thickness

The vessel details are 
MOC - SA 516 GR 70 
DIAMETER- 4020mm
LENGTH - 37 MTR
MDMT = - 50 Deg C to  + 250 Deg C 
SERVICE - Non lethal /No Hydrogen Service 

We are proposing Vessel length build up as per FURNACE LENGTH CAPACITY(24 m maximum) and one joint WITHOUT PWHT  ( JOINING PWHTed sections earlier at site )
Proposal - 
1.MOC - SA 516 GR 70 
2.BUTTERING - ENiCrFe2 on 24 m section end and other at 13 m section end)
3,PWHT (section PWHT - One of 24  length and other 13 m)
 of  - 620 Deg C - 125 MINUTES 
4.Bevel preparation 
5.NDT - DPT 
Welding at site ( 24 m section with 13 m section) - ENiCrFe2 OR E309 
6.NDT - DPT AND UT

Expert opinion please  and share experience if any 

Vishwas 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/bdca7c90-9d2b-4df4-a685-5e7745a76351n%40googlegroups.com.

Wednesday, October 27, 2021

[MW:32576] Heat Treatment of 25CRMo4

Dear Sir
Can you provide me with the actual holding time for heat treatment of rod with diameter of 170mm  as the material is 25CrMo4  
i need to apply hardening at 840C but i don't know the appropriate holding time matching with the diameter of 170mm
Thanks in advance

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/fae61d6b-5a88-405d-b9ce-5c68c00e4356n%40googlegroups.com.

Monday, October 25, 2021

Re: [MW:32575] Cladding UNS 32750 verification of consumable used

Send tabular excel sheet with material MOCs and type of joint .
Address service conditions such as 
temperature ,corrosion atmosphere ,

regards 

On Mon, 25 Oct 2021, 08:44 Muhammad Azeem, <azeem7999@gmail.com> wrote:
Dear Experts ,
I need your kind advise on priority basis as per below mentioned query raised by our vendor ..


We have considered the following filler wire for girth welding of various
combination. Pl confirm the same.
For serial number A & B : ERNiCrMo‐3 (UNS N06625)
For serial number C : ER 2553 (UNS 39553).
A. Carbon Steel (P1 Gr 2) with UNS S32750 CRA Overlay to UNS S32750(D.S.S)
Solid Alloy Branch connection
B. Carbon Steel (P1 Gr 2) with UNS S32750 CRA Overlay to Carbon Steel (P1 Gr 2)
with UNS S32750 CRA Overlay.
C. UNS S32750 (D.S.S) Solid Alloy Girth welded Joints.


My Suggestion 
the suitable filler wire.
ERNiCrMo‐3 (UNS N06625) / ERNiCrMo‐8 (UNS N06975) is
acceptable to weld for serial
number A & B. with reference to
corrosion 

ER 2553 (UNS 39553)  / ER 309LMO  is
acceptable to use for serial
number C
if only PREN value of
weldment is more than 42

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/439c3117-485d-45fa-a059-2ae8dd018466n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADder3O3DnvSQGM9biQAcGZ5dsX-oqXpVbpwK6-K7XVqJdP_zA%40mail.gmail.com.

[MW:35738] ASME IX WPS Qualification Query: GTAW + FCAW with Multiple PQRs

Dear Welding Experts, I'm currently preparing a Welding Procedure Specification (WPS) and have encountered a request to qualify a GTAW +...