[MW:34163] IGC TEST FOR FILLER WIRE AND ELECTRODE.

Dear all,

How to prepare the test piece for IGC Test for filler wire and electrode...? where is given the detail about test piece preparation detail....

IGC TEST procedure as per  ASTM A262 PRACTICE-E


Thanks and regards
Sujit

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFonYWMnBmkYK9JXu5xvekayhyfXu1OE%2Bg_wmTpfiiu3EeHOOg%40mail.gmail.com.

Re: [MW:34163] impact test requirement

Dear vishwas sir,

Please find below reply.


What is the MDMT?----(-45°C @ 10 bar(g))
What is the Welding process?----(GTAW)
What is consumable? ----(ER308L)
Is this consumable is perused tested?( NO NOT TESTED)



Best Regards.
sujit


On Fri, 28 Apr 2023 at 21:44, Vishwas Keskar <vvkeskar123@gmail.com> wrote:
What is the MDMT?
What is the Welding process?
What is consumable?
Is this consumable is perused tested?

 
Go the UHA 51 - There are exemptions to SS consumables .
Pl go thr it .
I am sure these will get exempted 

Thanks 
Vishwas
IWE 


Sent from my iPhone

On 28-Apr-2023, at 4:28 PM, 'james gerald' via Materials & Welding <materials-welding@googlegroups.com> wrote:


1. MDMT
2. Applicable Design code to determine the exemption
3. Welding code such as ASME Sec.IX

Normally supplementary PQR for Hardness and Impact is permitted

Thanks & Regards

J.Gerald Jayakumar



On Friday, 28 April, 2023 at 04:07:48 pm IST, Rameshbabu B <rameshbabu.b@zetwerk.com> wrote:


Impact test temperature?

On Fri, 28 Apr 2023 at 15:44, sujit kumar <sujitkumar19942@gmail.com> wrote:
Dear all,

if we have already qualified WPS for  P no 8 to P no 8 . then now we have  the requirement of the impact test. what to do? since it is a supplementary essential requirement. so may i  prepare test piece for the impact test and attached this impact test report to previous wps...?



Regards.
sujit

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFonYWMLtSp8eEQ-4e4NwJTN_PJC72zwr-JSNy5ghOES%3Dwz7VQ%40mail.gmail.com.
--
Regards
Ramesh Babu Balaram
Head QA/QC
Zetwerk Manufacturing Businesses Private Limited
Mobile: +91 98 4 053 13 55

>>>DONATE NOW<<<
SUPPORT ZETWERK'S CAMPAIGN TO FEED THE VURNERABLE MIGRANT FACTORY WORKER POPULATION.
Contribute generously. Each donation will go towards essential ration kits.
Let's come together as a nation so that they don't have to go hungry

This information may be confidential and/or privileged. Use of this information by anyone other than the intended recipient is prohibited. If you receive this in error, please inform the sender and remove any record of this message

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHJfB2keMW%3D8RZdUGKinM%3De3z4W3V82%3DrmXFTwtsw9TtXD85RA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1170775803.711426.1682679001664%40mail.yahoo.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/EE1B29CE-80BE-4DA2-8B0F-9FCC2B50AF20%40gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFonYWPMvdf%3Def75v_yhPSs%3DvE0VuE%2BXs4_92rZrxSa6k0uXrQ%40mail.gmail.com.

Friday, April 28, 2023

Re: [MW:34161] impact test requirement

What is the MDMT?
What is the Welding process?
What is consumable?
Is this consumable is perused tested?

 
Go the UHA 51 - There are exemptions to SS consumables .
Pl go thr it .
I am sure these will get exempted 

Thanks 
Vishwas
IWE 


Sent from my iPhone

On 28-Apr-2023, at 4:28 PM, 'james gerald' via Materials & Welding <materials-welding@googlegroups.com> wrote:


1. MDMT
2. Applicable Design code to determine the exemption
3. Welding code such as ASME Sec.IX

Normally supplementary PQR for Hardness and Impact is permitted

Thanks & Regards

J.Gerald Jayakumar



On Friday, 28 April, 2023 at 04:07:48 pm IST, Rameshbabu B <rameshbabu.b@zetwerk.com> wrote:


Impact test temperature?

On Fri, 28 Apr 2023 at 15:44, sujit kumar <sujitkumar19942@gmail.com> wrote:
Dear all,

if we have already qualified WPS for  P no 8 to P no 8 . then now we have  the requirement of the impact test. what to do? since it is a supplementary essential requirement. so may i  prepare test piece for the impact test and attached this impact test report to previous wps...?



Regards.
sujit

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFonYWMLtSp8eEQ-4e4NwJTN_PJC72zwr-JSNy5ghOES%3Dwz7VQ%40mail.gmail.com.
--
Regards
Ramesh Babu Balaram
Head QA/QC
Zetwerk Manufacturing Businesses Private Limited
Mobile: +91 98 4 053 13 55

>>>DONATE NOW<<<
SUPPORT ZETWERK'S CAMPAIGN TO FEED THE VURNERABLE MIGRANT FACTORY WORKER POPULATION.
Contribute generously. Each donation will go towards essential ration kits.
Let's come together as a nation so that they don't have to go hungry

This information may be confidential and/or privileged. Use of this information by anyone other than the intended recipient is prohibited. If you receive this in error, please inform the sender and remove any record of this message

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHJfB2keMW%3D8RZdUGKinM%3De3z4W3V82%3DrmXFTwtsw9TtXD85RA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1170775803.711426.1682679001664%40mail.yahoo.com.

[MW:34161] Re: Suitable Welding Electrodes

For SA333-6 you can utilize the E7018-1
For A350-LF3 E8018-C3 is a good choice
for others, I have to investigate the material properties.

On Thursday, April 27, 2023 at 10:58:49 PM UTC-4 amso...@gmail.com wrote:
  Dear Experts,

Please suggest us the suitable electrode to weld the SA 537 Class1, SA 333 Grade 6, SA350 Gr.LF3 and SA 420 WPL9 with the Impact temperature at -60 Deg.C

Also Shell Thickness of SA 537 Class1 is 12mm & 16mm. Hence is this vessel required PWHT

I have chosen below electrode to weld these materials.

E8018-C3
ER80S-Ni1

E81T5-Ni3C

E81T5-Ni2C

Requesting expert opinions in these regards

Thanks and Regards,

MS


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/5b3f549e-1288-43f9-9305-898fe348db68n%40googlegroups.com.

Re: [MW:34159] impact test requirement

Supplimentary essential variable meant essential when impact test is required.. means requalification of PQR 

On Fri, Apr 28, 2023, 16:18 sujit kumar <sujitkumar19942@gmail.com> wrote:
-50 degree celcius

On Fri, Apr 28, 2023, 16:07 Rameshbabu B <rameshbabu.b@zetwerk.com> wrote:
Impact test temperature?

On Fri, 28 Apr 2023 at 15:44, sujit kumar <sujitkumar19942@gmail.com> wrote:
Dear all,

if we have already qualified WPS for  P no 8 to P no 8 . then now we have  the requirement of the impact test. what to do? since it is a supplementary essential requirement. so may i  prepare test piece for the impact test and attached this impact test report to previous wps...?



Regards.
sujit

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFonYWMLtSp8eEQ-4e4NwJTN_PJC72zwr-JSNy5ghOES%3Dwz7VQ%40mail.gmail.com.
--
Regards
Ramesh Babu Balaram
Head QA/QC
Zetwerk Manufacturing Businesses Private Limited
Mobile: +91 98 4 053 13 55

>>>DONATE NOW<<<
SUPPORT ZETWERK'S CAMPAIGN TO FEED THE VURNERABLE MIGRANT FACTORY WORKER POPULATION.
Contribute generously. Each donation will go towards essential ration kits.
Let's come together as a nation so that they don't have to go hungry

This information may be confidential and/or privileged. Use of this information by anyone other than the intended recipient is prohibited. If you receive this in error, please inform the sender and remove any record of this message

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHJfB2keMW%3D8RZdUGKinM%3De3z4W3V82%3DrmXFTwtsw9TtXD85RA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFonYWOeQ00qqVJws787WXWCOYcOP9F9k0Q1VdnNk7X%3D%2BGRAAg%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAGAT7zfNz14kjz_sAABKcyi%3DC4OOhuz-DG%3Dg-jdN4fkJ%2B4nmDw%40mail.gmail.com.

Re: [MW:34158] impact test requirement

This will get exempted according to UHA 51.

Still, if you wanted to qualify with an impact test refer below

1. Existing PQR parameters should follow for qualification.
2. Perform an Impact test on the specific temperature and support the results.

Regards

Ramesh Babu Balaram

General Manager - Corporate Quality

84/1, Vaishnavi Sovereign, Green Glen Layout, Bellandur, Bengaluru-560103


M 9840531355 E rameshbabu.b@zetwerk.com  W zetwerk.com

Graphical user interface    Description automatically generated

App Green Footer Image Please consider your environmental responsibility. Before printing this e-mail message, ask yourself whether you really need a hard copy.




On Fri, Apr 28, 2023 at 4:18 PM sujit kumar <sujitkumar19942@gmail.com> wrote:
-50 degree celcius

On Fri, Apr 28, 2023, 16:07 Rameshbabu B <rameshbabu.b@zetwerk.com> wrote:
Impact test temperature?

On Fri, 28 Apr 2023 at 15:44, sujit kumar <sujitkumar19942@gmail.com> wrote:
Dear all,

if we have already qualified WPS for  P no 8 to P no 8 . then now we have  the requirement of the impact test. what to do? since it is a supplementary essential requirement. so may i  prepare test piece for the impact test and attached this impact test report to previous wps...?



Regards.
sujit

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFonYWMLtSp8eEQ-4e4NwJTN_PJC72zwr-JSNy5ghOES%3Dwz7VQ%40mail.gmail.com.
--
Regards
Ramesh Babu Balaram
Head QA/QC
Zetwerk Manufacturing Businesses Private Limited
Mobile: +91 98 4 053 13 55

>>>DONATE NOW<<<
SUPPORT ZETWERK'S CAMPAIGN TO FEED THE VURNERABLE MIGRANT FACTORY WORKER POPULATION.
Contribute generously. Each donation will go towards essential ration kits.
Let's come together as a nation so that they don't have to go hungry

This information may be confidential and/or privileged. Use of this information by anyone other than the intended recipient is prohibited. If you receive this in error, please inform the sender and remove any record of this message

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHJfB2keMW%3D8RZdUGKinM%3De3z4W3V82%3DrmXFTwtsw9TtXD85RA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFonYWOeQ00qqVJws787WXWCOYcOP9F9k0Q1VdnNk7X%3D%2BGRAAg%40mail.gmail.com.

This information may be confidential and/or privileged. Use of this information by anyone other than the intended recipient is prohibited. If you receive this in error, please inform the sender and remove any record of this message

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHJfB2nbF7Ypkvntj_XxmsxnvHXiO-siLoHWvY4NXDHiw9j%3D%3DA%40mail.gmail.com.

Re: [MW:34160] impact test requirement

1. MDMT
2. Applicable Design code to determine the exemption
3. Welding code such as ASME Sec.IX

Normally supplementary PQR for Hardness and Impact is permitted

Thanks & Regards

J.Gerald Jayakumar



On Friday, 28 April, 2023 at 04:07:48 pm IST, Rameshbabu B <rameshbabu.b@zetwerk.com> wrote:


Impact test temperature?

On Fri, 28 Apr 2023 at 15:44, sujit kumar <sujitkumar19942@gmail.com> wrote:
Dear all,

if we have already qualified WPS for  P no 8 to P no 8 . then now we have  the requirement of the impact test. what to do? since it is a supplementary essential requirement. so may i  prepare test piece for the impact test and attached this impact test report to previous wps...?



Regards.
sujit

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFonYWMLtSp8eEQ-4e4NwJTN_PJC72zwr-JSNy5ghOES%3Dwz7VQ%40mail.gmail.com.
--
Regards
Ramesh Babu Balaram
Head QA/QC
Zetwerk Manufacturing Businesses Private Limited
Mobile: +91 98 4 053 13 55

>>>DONATE NOW<<<
SUPPORT ZETWERK'S CAMPAIGN TO FEED THE VURNERABLE MIGRANT FACTORY WORKER POPULATION.
Contribute generously. Each donation will go towards essential ration kits.
Let's come together as a nation so that they don't have to go hungry

This information may be confidential and/or privileged. Use of this information by anyone other than the intended recipient is prohibited. If you receive this in error, please inform the sender and remove any record of this message

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHJfB2keMW%3D8RZdUGKinM%3De3z4W3V82%3DrmXFTwtsw9TtXD85RA%40mail.gmail.com.

Re: [MW:34157] impact test requirement

-50 degree celcius

On Fri, Apr 28, 2023, 16:07 Rameshbabu B <rameshbabu.b@zetwerk.com> wrote:
Impact test temperature?

On Fri, 28 Apr 2023 at 15:44, sujit kumar <sujitkumar19942@gmail.com> wrote:
Dear all,

if we have already qualified WPS for  P no 8 to P no 8 . then now we have  the requirement of the impact test. what to do? since it is a supplementary essential requirement. so may i  prepare test piece for the impact test and attached this impact test report to previous wps...?



Regards.
sujit

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFonYWMLtSp8eEQ-4e4NwJTN_PJC72zwr-JSNy5ghOES%3Dwz7VQ%40mail.gmail.com.
--
Regards
Ramesh Babu Balaram
Head QA/QC
Zetwerk Manufacturing Businesses Private Limited
Mobile: +91 98 4 053 13 55

>>>DONATE NOW<<<
SUPPORT ZETWERK'S CAMPAIGN TO FEED THE VURNERABLE MIGRANT FACTORY WORKER POPULATION.
Contribute generously. Each donation will go towards essential ration kits.
Let's come together as a nation so that they don't have to go hungry

This information may be confidential and/or privileged. Use of this information by anyone other than the intended recipient is prohibited. If you receive this in error, please inform the sender and remove any record of this message

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHJfB2keMW%3D8RZdUGKinM%3De3z4W3V82%3DrmXFTwtsw9TtXD85RA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFonYWOeQ00qqVJws787WXWCOYcOP9F9k0Q1VdnNk7X%3D%2BGRAAg%40mail.gmail.com.

Re: [MW:34156] impact test requirement

Impact test temperature?

On Fri, 28 Apr 2023 at 15:44, sujit kumar <sujitkumar19942@gmail.com> wrote:
Dear all,

if we have already qualified WPS for  P no 8 to P no 8 . then now we have  the requirement of the impact test. what to do? since it is a supplementary essential requirement. so may i  prepare test piece for the impact test and attached this impact test report to previous wps...?



Regards.
sujit

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFonYWMLtSp8eEQ-4e4NwJTN_PJC72zwr-JSNy5ghOES%3Dwz7VQ%40mail.gmail.com.
--
Regards
Ramesh Babu Balaram
Head QA/QC
Zetwerk Manufacturing Businesses Private Limited
Mobile: +91 98 4 053 13 55

>>>DONATE NOW<<<
SUPPORT ZETWERK'S CAMPAIGN TO FEED THE VURNERABLE MIGRANT FACTORY WORKER POPULATION.
Contribute generously. Each donation will go towards essential ration kits.
Let's come together as a nation so that they don't have to go hungry

This information may be confidential and/or privileged. Use of this information by anyone other than the intended recipient is prohibited. If you receive this in error, please inform the sender and remove any record of this message

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHJfB2keMW%3D8RZdUGKinM%3De3z4W3V82%3DrmXFTwtsw9TtXD85RA%40mail.gmail.com.

[MW:34155] impact test requirement

Dear all,

if we have already qualified WPS for  P no 8 to P no 8 . then now we have  the requirement of the impact test. what to do? since it is a supplementary essential requirement. so may i  prepare test piece for the impact test and attached this impact test report to previous wps...?



Regards.
sujit

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFonYWMLtSp8eEQ-4e4NwJTN_PJC72zwr-JSNy5ghOES%3Dwz7VQ%40mail.gmail.com.

Thursday, April 27, 2023

[MW:34153] Suitable Welding Electrodes

  Dear Experts,

Please suggest us the suitable electrode to weld the SA 537 Class1, SA 333 Grade 6, SA350 Gr.LF3 and SA 420 WPL9 with the Impact temperature at -60 Deg.C

Also Shell Thickness of SA 537 Class1 is 12mm & 16mm. Hence is this vessel required PWHT

I have chosen below electrode to weld these materials.

E8018-C3
ER80S-Ni1

E81T5-Ni3C

E81T5-Ni2C

Requesting expert opinions in these regards

Thanks and Regards,

MS


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/3290864a-54a9-498f-abf2-a682371cc357n%40googlegroups.com.

[MW:34152] Kind Request for Sample WPS

Dear Team,

Good Day

Kindly provide below detailed sample WPS.

Material = S355J2 to 30CrNiMo8
Welding Process = SMAW
Standard = AWS D1.1


Thanks & Regards,

 

 D. Prabu 

India - 637408.

 Mob.: 0091-8428254475

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADJABCax%2BN5G7fgC7VhTh%3D8fGGF8r4rqPab9Cm%2Be6Bw6ScWsuA%40mail.gmail.com.

Wednesday, April 26, 2023

Re: [MW:34149] Re: Advise for Weld defects during SAW Welding

Dear experts thank you for your valuable advises. 

The used consumables are
Wire : Cordiff 357 SA (Cr, Ni, Mo alloyed Tubular wire) Make - Diffusion
Flux: Supershield SS Flux ( Basic Flux, Neutral behaviour in terms of C, Cr, Ni & Mo pick-up or burn out)  Make: Super Alloys & Metals

Regards,
On Wednesday, 26 April 2023 at 10:37:39 UTC+5:30 RANEESH PK wrote:
because of very  high traveling speed and long weld bead. 

On Wed, 26 Apr 2023 at 7:04 AM Mehrab Chakoshkar <mehrab.c...@gmail.com> wrote:
Hi
First, you should give us sufficient information such as the AWS Classification, the wire and flux name, and the ASTM name of the material.
second, seemingly your welding speed has been high, I can see the long beads in the welding direction.
third, sticking the slag usually happens when the A is too high and the cause of porosity usually is moisture in the flux, have you baked the flux before use?
Mehrab
On Tuesday, April 25, 2023 at 7:40:09 AM UTC-4 SMM wrote:
Dear Experts, 

There are few issues found during SAW weld  cladding at site and are highlighted in the report. Please find attached report.

I have a few questions
1. Reason for such issue to occur. 
2. Is the issue of Flux (neutral basic flux) or Flux cored wire used in the process.
3. Please advise how can this be sorted out.

Thank you,
George

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/f0d1d079-bd34-40d1-add5-1e7196809f34n%40googlegroups.com.

Re: [MW:34149] EXCEL SHEET : WELD CONSUMABLE QUANTITY CALCULATOR

Dear Sir,

Thanks for sharing the file.
It is password protected, do you have the password

Thank You & Regards
Williams P Wilson
+968-94600828
QA/QC Engineer
Please consider the environment before printing this message


On Fri, Nov 2, 2018 at 12:28 PM 'Karthik' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Hi,
The attached file might be useful to you.

Thanks& Regards,

 

(Karthik)

Karthikeyan.S

QA/QC Manager
Agon Pacific Co.,Ltd.
M: +66-655-174-397, +66-892-512-282

E-mail : karthik6684@yahoo.com



On Friday, November 2, 2018, 1:41:24 PM GMT+7, MITHLESH <qa.ap2@jshl.in> wrote:


HI SIR,
In attached file, ID means inch dia? and another thing is deposition rate of SAW not given. is it not applicable for SAW? 

On Thursday, November 5, 2015 at 10:39:05 AM UTC+5:30, Karthik wrote:
 Hi, 
The attached file might be useful to you
Thanks& Regards,
 
(Karthik)
QA/QC Manager 
CMI-Thai Services Co.,Ltd. 
50/35 Sermsuwan Road,Tambol Maptaphut 
Amphur Muang Rayong,Rayong 21150
Thailand
www.cmi-services.com 
Tel : +66 38 691 390-2 ext.103 
Fax : +66 38 682 338 
Mobile: +66 892512282 
E-mail : karth...@cmi-services.com
               Karth...@yahoo.com



On Wednesday, November 4, 2015 4:56 PM, waqas suleman <waqas....@gmail.com> wrote:


Dear Members,

I am also waiting for the same below requested file.

Regards,

Waqas Suleman
Mob. 00966 59 359 0798

On Tue, Nov 3, 2015 at 10:21 AM, Vikas Bhandari <vikas.bh...@gmail.com> wrote:
Hi

Can anyone share a standard excel sheet  for pipe butt weld consumable quantity calculation?

Many thanks

Best regards

Vb
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@ googlegroups.com.
To post to this group, send email to material...@ googlegroups.com.
Visit this group at http://groups.google.com/ group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/ msgid/materials-welding/ CACpSjOn%3DhNb3z324Ci-% 3D94bUSjpD7oVQUJBeWVokThmCi0GL %2Bg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/ optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@ googlegroups.com.
To post to this group, send email to material...@ googlegroups.com.
Visit this group at http://groups.google.com/ group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/ msgid/materials-welding/ CAKhANKjVn2-NoB%3D9nRZP2Fm% 3D8LyJWNoXzyZrpR_RAgvNefHRAQ% 40mail.gmail.com.
For more options, visit https://groups.google.com/d/ optout.






--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHBxnQ4cGXQzCwBJmOoSX5gwKFL5WoWk-f3t0vjtu0OOe7GCaw%40mail.gmail.com.

Re: [MW:34151] Re: Advise for Weld defects during SAW Welding

Thank you for the replies experts.

Wire used: CORDIFF 357 SA (Cr, Ni, and Mo alloyed tubular wire) Make - Diffusion
Flux used: SUPERSHIELD SS Flux Make - Super Alloys and metals (data sheet attached)

Regards,
On Wednesday, 26 April 2023 at 10:37:39 UTC+5:30 RANEESH PK wrote:
because of very  high traveling speed and long weld bead. 

On Wed, 26 Apr 2023 at 7:04 AM Mehrab Chakoshkar <mehrab.c...@gmail.com> wrote:
Hi
First, you should give us sufficient information such as the AWS Classification, the wire and flux name, and the ASTM name of the material.
second, seemingly your welding speed has been high, I can see the long beads in the welding direction.
third, sticking the slag usually happens when the A is too high and the cause of porosity usually is moisture in the flux, have you baked the flux before use?
Mehrab
On Tuesday, April 25, 2023 at 7:40:09 AM UTC-4 SMM wrote:
Dear Experts, 

There are few issues found during SAW weld  cladding at site and are highlighted in the report. Please find attached report.

I have a few questions
1. Reason for such issue to occur. 
2. Is the issue of Flux (neutral basic flux) or Flux cored wire used in the process.
3. Please advise how can this be sorted out.

Thank you,
George

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/19b59249-3500-4de4-beb3-792f09bf2b1fn%40googlegroups.com.

Re: [MW:34148] Re: Advise for Weld defects during SAW Welding

because of very  high traveling speed and long weld bead. 

On Wed, 26 Apr 2023 at 7:04 AM Mehrab Chakoshkar <mehrab.chakoshkar@gmail.com> wrote:
Hi
First, you should give us sufficient information such as the AWS Classification, the wire and flux name, and the ASTM name of the material.
second, seemingly your welding speed has been high, I can see the long beads in the welding direction.
third, sticking the slag usually happens when the A is too high and the cause of porosity usually is moisture in the flux, have you baked the flux before use?
Mehrab
On Tuesday, April 25, 2023 at 7:40:09 AM UTC-4 SMM wrote:
Dear Experts, 

There are few issues found during SAW weld  cladding at site and are highlighted in the report. Please find attached report.

I have a few questions
1. Reason for such issue to occur. 
2. Is the issue of Flux (neutral basic flux) or Flux cored wire used in the process.
3. Please advise how can this be sorted out.

Thank you,
George

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/fd4287e9-aa49-422c-9837-11ca2bb44595n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAERXeWneJgDxMVeUsTsqcDys1ShP4Ux3i9PhEssBPPmczBbpgg%40mail.gmail.com.

Tuesday, April 25, 2023

[MW:34147] Re: Advise for Weld defects during SAW Welding

Hi
First, you should give us sufficient information such as the AWS Classification, the wire and flux name, and the ASTM name of the material.
second, seemingly your welding speed has been high, I can see the long beads in the welding direction.
third, sticking the slag usually happens when the A is too high and the cause of porosity usually is moisture in the flux, have you baked the flux before use?
Mehrab
On Tuesday, April 25, 2023 at 7:40:09 AM UTC-4 SMM wrote:
Dear Experts, 

There are few issues found during SAW weld  cladding at site and are highlighted in the report. Please find attached report.

I have a few questions
1. Reason for such issue to occur. 
2. Is the issue of Flux (neutral basic flux) or Flux cored wire used in the process.
3. Please advise how can this be sorted out.

Thank you,
George

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/fd4287e9-aa49-422c-9837-11ca2bb44595n%40googlegroups.com.

[MW:34146] RE: 34145] Advise for Weld defects during SAW Welding

What's the wire & flux make  being used. Do not provide the AWS grade alone , specify the make also. That's important.

 

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Independent Welding & Metallurgical Engineering Specialist

Consultant: SNC Lavalin Inc. (Nuclear &Non-Nuclear)

Saudi Aramco Approved Designated Project Welding Engineer (DPWR)

Qatar Petroleum Approved, SME-Materials & Corrosion Engineering.

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@rogers.com,pradip.goswami@gmail.com

Cell/Whasapp:1-905-9793232

 

From: materials-welding@googlegroups.com <materials-welding@googlegroups.com> On Behalf Of SMM
Sent: April 25, 2023 7:38 AM
To: Materials & Welding <materials-welding@googlegroups.com>
Subject: [MW:34145] Advise for Weld defects during SAW Welding

 

Dear Experts, 

 

There are few issues found during SAW weld  cladding at site and are highlighted in the report. Please find attached report.

 

I have a few questions

1. Reason for such issue to occur. 

2. Is the issue of Flux (neutral basic flux) or Flux cored wire used in the process.

3. Please advise how can this be sorted out.

 

Thank you,

George

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/c92d0a0d-f589-47eb-8def-01c5e040a3b2n%40googlegroups.com.


Virus-free.www.avg.com

[MW:34145] Advise for Weld defects during SAW Welding

Dear Experts, 

There are few issues found during SAW weld  cladding at site and are highlighted in the report. Please find attached report.

I have a few questions
1. Reason for such issue to occur. 
2. Is the issue of Flux (neutral basic flux) or Flux cored wire used in the process.
3. Please advise how can this be sorted out.

Thank you,
George

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/c92d0a0d-f589-47eb-8def-01c5e040a3b2n%40googlegroups.com.

Monday, April 24, 2023

Re: [MW:34143] USE of PQR of GTAW+SMAW for new WPS GTAW process only.

Dear Ajay

Yes, you can use the GTAW Process from PQR GTAW+SMAW as long as the essential variable PQR will cover into new WPS.
for thickness range for GTAW Process, refer to Table QW-451.1 of ASME Sect IX, it should be 5mm ~ 14mm

Hopely the above can answer your question

Best regards
Kurniatullah, IWE

On Wed, Apr 12, 2023 at 10:02 AM Ajay Kaipuram <ajaykdas144@gmail.com> wrote:
Hi,

I have a PQR with a thickness range of 7mm (GTAW)+ 14.94mm (SMAW) for the groove joint. Can I prepare a new WPS for the job with a 5.08 mm thick groove joint for the GTAW process only? If yes, what thickness range can I mention in the WPS?

Regards,
Ajay

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b7cd158a-7548-4229-9ead-c6c37bed3548n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFo4ueq4VobgaLyigwfpRUTSjEyFD32YaWzEkW90DiDhoWvnjw%40mail.gmail.com.

Re: [MW:35737] Bend Test and Tensile Test failed for ET45 Micro Welded Coupon

Hi As its %elongation is very low  Better try buttering on jt surrace with ductile consumable like pure Ni i. E Ni1 And later weld jt with c...