[MW:3842] RE: 3835] SA387 Gr.11 Cl.2 material welding.

Dear all

With regard to Mr. P.Rao question :

1-      Use EB2 materials group.

2-      690 ±14 °C is better range for PWHT.

3-      Pay attention to 149 °C preheat and a suitable post heating.

4-      Check edges and bevels for hardness before welding.

5-      Check PWHT plus any intermediate treatment ( above 482°C) on LMP.

 

Best Regards

 

A.  Varmazyar

 

MSA-Red.png

 

MSA -Welding Engineering Department

Msa,Arak,Markazi,IRAN – P.O. 148

Tel.: +988612172725~6

Fax: +988612172702

 

 

------------------------------------------------------------

 

 

 

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of PAMULA
Sent: Monday, December 14, 2009 6:56 PM
To: materials-welding@googlegroups.com
Subject: [MW:3835] SA387 Gr.11 Cl.2 material welding.

 


Dear all,

Can any body have experiance on welding of SA387 Gr.11 Cl.2 (1 1/4Cr-1/5 Mo)material with E8018-B3L, ER80S-B3L, EB3 type welding consumables(2 1/4 Cr-1Mo).

Higher composition consumables (B3L) are recommended?

Is there any change in PWHT is required as compared to standard PWHT cycle for SA387 Gr.11 Cl.2 material as per ASME Div.1.

Pl. share experiance on welding of subject material.

( Design Code : ASME div.1
MDMT : 0 Deg.C
Impact : 50/40)

regards

P.Rao