Skip to main content

Re: [MW:3683] Re: Cold form dish

Dear Anant,

5% fibre elongation is the limit for Carbon and low alloy steel. For stainless steel it is 15-20%. We have to refere UHA-44 and table UHA-44 where the requirement are clearly mentioned.

Hope this will help to make decision.

Regards.
C. K. Purohit
Eng-Tech Weld1
Sr Welding Inspector
 

2009/11/17 ANANT ONKAR <jointcross@hotmail.com>
Dear Pl. check what percentage elongation is coming while cold forming if it is more than 5 % you have to do heat treatment.
Regards
Anant 
 

From: AshokKumar@Zamilsteel.comDate: Mon, 16 Nov 2009 11:01:04 +0300
Subject: [MW:3666] Re: Cold form dish


Dear Devang Patel

 

                If u r doing cold forming no heat treatment is required for both CS & SS material

Regards

P.Asok Kumar

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Devang Patel
Sent: Monday, November 16, 2009 9:19 AM
To: materials-welding@googlegroups.com
Subject: [MW:3664] Cold form dish

 

Can any one know about SA-240 type 304LN or X2CrNiN 18-10(1.4311)material?

If we make cold form dish than heat treatment is required or not??

 

 

Regards,
Devang Patel | Manager Engineering
Inox India Ltd. | 4th Floor, ABS Tower, Old Padra Road, Vadodara. Guj. India.
Voice: + 91-265-3056100 ext. 392 | Fax: +91-265-2341449 | Mobile: +91 9879803401
Email: devangp@inoxindia.com | web: www.inoxindia.com

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Anonymous said…
It is very interesting for me to read that article. Thank author for it. I like such themes and anything connected to them. I would like to read more on that blog soon.
Anonymous said…
Pretty interesting blog you've got here. Thanx for it. I like such topics and anything that is connected to this matter. BTW, try to add some photos :).

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...