Sorry I didn't mention, for my previous mail  I refer ASME section V Edition 2007 addenda 2008

Regards

Bharat B. Gole





From: bharatgole@hotmail.com
To: materials-welding@googlegroups.com
Subject: RE: [MW:3731] NDT procedure qualification
Date: Wed, 25 Nov 2009 16:48:14 +0530


If you refer ASME V  clause  T522.1,T721.2 & T621.2 for UT,MT & PT respectively then you will find that when procedure qualification is specified by the referncing code section(i.e construction code...ASME VIII, 31.3 etc) , change of requirment in relevant table ( ASME V )identifed as an essential variable shall require requlification of written procedure by demonstration.

Where as per ASME V clause T 221.2 for RT - Only demonstration of density & image quality requirements as per written procedure  on production or technique radiograph shall be considered satisfactory evidence of compliance of that procedure.

Suppose if you are qualifying welder by radiography then even written procedure is also not required as per QW 190 Only demonstration of density & image quality requirements on production or technique radiograph shall be considered satisfactory evidence of compliance with article 2 of section V.

I think its more clear now. If you come across with some clients specification then you may have to demonstrate the NDT procedures beside abovsaid code requiremnts.

Regards

Bharat B. Gole

 






To: materials-welding@googlegroups.com
Subject: Re: [MW:3731] NDT procedure qualification
From: Vinayak_Kale@lntenc.com
Date: Wed, 25 Nov 2009 08:56:06 +0530


Good Morning ,

Basically  NDT procedures are drafted in line with specific codes for example ASME Sec V which is universally adopted. If client insist or raise any doubt than only we have to demonstrate



Thanks & Best Regards,

Vinayak Kale
E & C  DIv. QA & I , OGSP
Larsen And Toubro Ltd
Powai , Mumbai
vinayak_kale@lntenc.com
Ph No.+91- 67053805/3685
Fax No. +91-67051988
(M) - + 91 9892743803



"K.M Hrishikesan" <hrishikm07@gmail.com> 11/24/2009 06:21 PM
Please respond to
materials-welding@googlegroups.com


To
materials-welding@googlegroups.com
cc

Subject
[MW:3725] NDT procedure qualification







Is it mandatory to demonstrate NDT procedure qualification before applying in the actual job? If so, please give the code/standard reference.
 
Regards
Hrishi --
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


Disclaimer :This email and any files transmitted with it are intended solely for the use of the addressee(s) only and may contain confidential and/or privileged information. If you are not the addressee, then this message is not intended for you and be advised that you have received this email in error and that any use , dissemination , forwarding, printing or copying of this email is strictly prohibited. In such case please notify the sender and delete this email and any attachments with it from your system immediately.Receipt of this email by you shall not give rise to any liability on the part of Larsen & Toubro Limited


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


http://windows.microsoft.com/shop Find the right PC for you.

New Windows 7: Find the right PC for you. Learn more.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...