Without impact testing
1.5 to 16mm base metal thickness can be welded.
With impact testing
Any material combination can be welded within range of 10-16mm base metal thickness
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Sukamal Naskar
Sent: Monday, November 24, 2008 11:36 AM
To: materials-welding@googlegroups.com
Subject: [MW:1334] WPS combination of two PQRs
Friends,
Good afternoon. I need one help regarding one WPS, combination of two PQRs.
the 1st PQR is 8mm thick, with base material SA 516Gr.70 ( P No.1 Gr. 2) with SA 516 Gr.65 (P No.1 Gr.1). welded with full GTAW process , and is impact tested at -29 deg. C.2nd PQR is 10mm thick, with base material SA 516Gr.70 ( P No.1 Gr. 2) with SA 516 Gr.70 (P No.1 Gr.2). welded with full SMAW process , and is impact tested at -29 deg. C.
If we combine these two PQRs to make one WPS for the combination welding process GTAW & SMAW, will the base material thickness range will be 8 mm to 20mm ( with impact) and 1.5 mm to 20mm (without impact) ?
The deposited weld metal thickness for GTAW will be 16 mm max. and SMAW 20mm max. ( for both with / without impact)
And if the impact test is required at - 29 deg. C, can we use this WPS for all possible base material combinations ( P1 Gr.1 to P1Gr.1; P1 Gr2 to P1 Gr2 and P1 Gr.1 to P1 Gr.2) ??
Regards
--
Sukamal Naskar
MMHE ATB
+60177007205
Malaysia
--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---
Monday, November 24, 2008
[MW:1344] Re: 1334] WPS combination of two PQRs
Thanks for your responce.
Can you please let me know according to which clause of ASME Sec-IX, the base material thickness is 10mm to 16mm with impact . why not 8mm to 20mm ( combination of two PQRs)
Regards
On 11/24/08, Bathula Raghuram (Mumbai - PIPING) <R.Bathula@ticb.com> wrote:
Subscribe to:
Post Comments (Atom)
Re: [MW:35686] HDPE WPS
Refer ASME SEC IX There is separate chapter for Plastic welding . Based on that you have to prepare Sent from my iPhone On 21 Jun 2025, at...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-
Section I. PRINT READING 3-1. GENERAL a. Drawings . Drawing or sketching is a universal language used to convey all necessary information to...