Skip to main content

[MW:1341] Re: 1334] WPS combination of two PQRs

Pl see below and read care fully in between the lines

You need to check qualification range for T (base metal thickness) t (deposited metal thickness)


From: Sukamal Naskar [mailto:sukamalbecmet@gmail.com]
Sent: Monday, November 24, 2008 1:45 PM
To: Bathula Raghuram (Mumbai - PIPING)
Subject: Re: [MW:1336] RE: 1334] WPS combination of two PQRs

 

Thanks for your reply.

 But, QW-403.5   states that " .......... If, however , two or more qualification records have the same essential and supplementary essential variables, except that the base metals are assigned to different group numbers within the same P-Number, then the combination of base metals is also qualified."

It should have same essential and supplementary essential variables, one is GTAW and the other is SMAW, hence combination can be used only GTAW and not for GT+SM

 

Also QW-403.6 states only for the lower limit of the base metal thickness if impact required, and in this case for the 8mm thick plate it qualifies from 8mm to 16mm (QW-403.6 & QW-451.1) & for 10 mm it will qualify 10mm to 20mm.( QW-403.6 & QW-451.1). So if we combine both the PQRs, then why not the base metal thickness range from 8mm to 20 mm?

Here you need to check the limits for T and t separately; QW 403.6 does n’t states about t,

For e.g. even if ur depositing only root with GTAW you can’t deposit it on a 20mm plate.

QW-200.2(f), has given one example for combination of two PQRs to get the base metal thickness ranges, can it be followed?

 It also states about supplementary essential variable is n’t it?

 

On 11/24/08, Bathula Raghuram (Mumbai - PIPING) <R.Bathula@ticb.com> wrote:

QW403.5 and 403.6


From: Sukamal Naskar [mailto:sukamalbecmet@gmail.com]
Sent: Monday, November 24, 2008 1:19 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:1336] RE: 1334] WPS combination of two PQRs

 Thanks for your responce.

 Can you please let me know according to which clause of ASME Sec-IX, the base material thickness is 10mm to 16mm with impact . why not 8mm to 20mm ( combination of two PQRs)

 Regards

 On 11/24/08, Bathula Raghuram (Mumbai - PIPING) <R.Bathula@ticb.com> wrote:

With impact testing

Any material combination can be welded within range of 10-16mm base metal thickness

Sorry, There was a mistake here P1G1 can’t be welded using SMAW process

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Bathula Raghuram (Mumbai - PIPING)
Sent: Monday, November 24, 2008 1:06 PM
To: materials-welding@googlegroups.com
Subject: [MW:1336] RE: 1334] WPS combination of two PQRs

 

Without impact testing

1.5 to 16mm base metal thickness can be welded.

With impact testing

Any material combination can be welded within range of 10-16mm base metal thickness

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Sukamal Naskar
Sent: Monday, November 24, 2008 11:36 AM
To: materials-welding@googlegroups.com
Subject: [MW:1334] WPS combination of two PQRs

 Friends,

Good afternoon. I need one help regarding one WPS, combination of two PQRs.
the 1st PQR is 8mm thick, with base material SA 516Gr.70 ( P No.1 Gr. 2) with SA 516 Gr.65 (P No.1 Gr.1). welded with full GTAW process , and is impact tested at -29 deg. C.

2nd PQR is 10mm thick, with base material SA 516Gr.70 ( P No.1 Gr. 2) with SA 516 Gr.70 (P No.1 Gr.2). welded with full SMAW process , and is impact tested at -29 deg. C.

If we combine these two PQRs to make one WPS for the combination welding process GTAW & SMAW, will the base material thickness range will be 8 mm to 20mm ( with impact) and 1.5 mm to 20mm (without impact) ?

The deposited weld metal thickness for GTAW will be 16 mm max. and SMAW 20mm max. ( for both with / without impact)

And if the impact test is required at - 29 deg. C, can we use this WPS for all possible base material combinations ( P1 Gr.1 to P1Gr.1; P1 Gr2 to P1 Gr2 and P1 Gr.1 to P1 Gr.2) ??

 Regards

Sukamal Naskar
MMHE ATB
+60177007205
Malaysia

  


--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...