Skip to main content

RE: [MW:9740] CS to SS welding

Dear Manpreet,

Please note the required details as per the following in RED colour:-

 

* Welding Process – GTAW for Root and Filling with SMAW.
* Thickness of the materials (Dissimilar weld ?) – 4.5mm.
* Welding Technique– String, cup size 6mm, multipass, single electrode.
* Preheat temp. – 20 degree C min.
* Heat Input– 0.95 to 1.19 KJ/mm.

With kind regards,

Vinod Kumar Kataria

GM - Operations

Bliss Anand Private Limited,

92B/93B Sector 5

IMT Manesar,Gurgaon,

National Capital Region Delhi.

India .

Phone : +91-124-4366000 (9 Lines)

Mobile Phone : +91-9560199004

Fax : +91-124-2290884

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of manpreet
Sent: Saturday, February 05, 2011 7:58 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:9737] CS to SS welding

 

Dear Vinod,

Ok then, I would like you to provide some more info.

* Welding Process
* Thickness of the materials (Dissimilar weld ?)
* Welding Technique
* Preheat temp.
* Heat Input

Changes may be required for above stated factors (in lieu of PQR) to overcome this problem.

Regards
Manpreet Singh



On Sat, 05 Feb 2011 01:15:21 +0530 "Vinod Kataria" wrote
>

Dear Manpreet,

Thanks for your valuable time. Please note we have qualified PQR using Filler 309L only but so many time we are getting more than 22 HRC which is not acceptable as per Nace MR 0175.

With kind regards,

Vinod Kumar Kataria

GM - Operations

Bliss Anand Private Limited,

92B/93B Sector 5

IMT Manesar,Gurgaon,

National Capital Region Delhi.

India .

Phone : +91-124-4366000 (9 Lines)

Mobile Phone : +91-9560199004

Fax : +91-124-2290884

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of manpreet
>Sent: Friday, February 04, 2011 3:17 PM
>To: materials-welding
>Subject: Re: [MW:9727] CS to SS welding

Dear Vinod,
>
>When welding Carbon steel to stainless steel, one should avoid formation of martensite by using overalloyed filler metal (309L) which willformAustenite even when cooling,a Preheatingand using Temper bead technique would also be helpfull to reduce Hardness,
>
>Considerationmust be given to reduce High Dilution by reducing Travel Speed, buttering the joint face, no SAW etc.
>
>Also refer to the Shaeffler Diagram to evaluate what kind of microstructue you would expect, with filler metal E309L, you can expect "Austenite with little ferrite".
>
>Regards
>Manpreet Singh
>
>
>
>On Fri, 04 Feb 2011 13:18:26 +0530 "Vinod Kataria" wrote
>>

Hi,

How to control the hardness for NACE MR 0175 application if we have to use A-105 flanges on SS-316 Chamber as PWHT cannot be done.

With kind regards,

Vinod Kumar Kataria

--
>>To post to this group, send email to materials-welding@googlegroups.com
>>To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>>
>

--
>To post to this group, send email to materials-welding@googlegroups.com
>To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
>To post to this group, send email to materials-welding@googlegroups.com
>To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...