Re: [MW:33297] Pickling and passivation need before painting SS surfaces

Pickling and passivation is  Not required  ,   because you are going for painting after completion of NDE but  for the process side (Accessible Root) you may need to perform if purging is not maintained properly. or any heat tints found unacceptable.
 
If you  painting is not involved ,  Yes, it is required to perform the  pickling and passivation of SS weldments 100% as due to heat generation  during welding the passivation layer will be damaged and may not be formed naturally, in general  Passivation will form naturally in air & it may take longer time to form for protection to occur. Before this period, passivation by using Chemicals may be carried out rapidly. as we are not checking for confirmation of the passivation layer formation. 

 refer any client specifications Ex. DEP 30.10.60.18 / ADNOC specifications about this requirements for stainless steels  welds 

Regards,
Srinuvasa Rao

On Tue, Jul 26, 2022 at 12:35 PM sajeed zaheer <sajeed7674@gmail.com> wrote:
ASTM A 380

On Tue, Jul 26, 2022 at 11:19 AM Anilkumar G <akg.nitt@gmail.com> wrote:
Dear Experts

Do we need pickling and passivation of SS surfaces before painting them? Could you please suggest any specification relevant this requirement?
The parts are SS cast valves requiring painting.

Regards
Anilkumar

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/754e0d61-54e1-420e-ae4b-f92593266f5en%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFycdMz9RbXVXteXk%2B3MvOj%3D%2B2ftw-bu-N9jAx1tsvtrz3L7Gw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHdRSONAmRhoaZnSZgQjndMMsC4WZ085EyncChWJXO3fDGdBiA%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...