Re: [MW:33267] Baking Electrods only one time, but how ?

Initial Baking of Low H2 electrodes will be performed by the Electrode Manufacture in their plant. What actually you perform in your shop is rebaking/Baking and please verify with the Client their terminology used in Specification.

After exposure for 4/8 Hours based on client specification and manufacturer recommendation rebaking to be done. Normally practice is to Dip the stub end side of the electrode in Paint (various colours for first rebake & second rebake). Inform the Store Keeper to distribute only minimum quantities of paint marked electrodes to welders while they collect the electrode in their quiver from Holding oven say 10 electrodes and instruct the welders to consume the paint marked electrodes first and in this way you can control the next rebake.

Thanks & Regards

J.Gerald Jayakumar



On Monday, 18 July, 2022 at 07:21:31 am GMT+4, Anilkumar G <akg.nitt@gmail.com> wrote:


The electrode baking shall be as per the consumable manufacturer recommendations. This can't be generalised, we all know.
If customer specification allows baking more than once, at the same time if the electrode manufacturer is also ok for baking a second time, you can do it. Go for it. 

On Sat, Jul 16, 2022 at 6:34 PM madheswaran s <madhes.sss@gmail.com> wrote:
Dear Experts, 

I have a question about baking of electrodes. spec or other says backing of electrodes only one time. Now my question is if i received electrodes carton box from manufacturer Like E7018 ok, If  baking the electodes then we maintain the elecrodes in holing oven the issuesd to welder for welding, If some electodes are not used , they are exposed in atmosperic condition about 8 hrs, In this case can i do baking again? or already once we backed the elecrode before issuing to welder, so we can't back again? because once only baking permitted. I dont know clear understand ? can anyone help this case.
 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/4b3918f2-ec32-4a7f-9d04-6ce30107b9dbn%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAKMJiNXjQqVFcrC5UxpCQS6KUED-CtWqfQDfjJP%2BVhHNv8QgEw%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...