Skip to main content

Re: [MW:33263] SA-516 Gr 70


Dear Kishore , 
consuamble selction is mainly depends on  Base metal  tensile properties , Specification and service requirements(Hardness and impact requiremnts). other facrtor also to be taken into considered in case if you wan to fo with different welding processes ,in your  case it is already SMAW process  and  base metrial is  SA 516 Gr 70 means minimum specified tensile strength is 70000psi /485 Mpa. while selecting consumable you need to consider the minimum specified stregth of the base metal not acutal tensilet stregth  specified in MTC , so the recommended  electode for this purpose is E7018 which satisfys the base mental strength requirement for impact requirements to be confirmed by manufaturer based on your project requiremnts, over matching consuambes are not required in this regard as many of the applications E7018/E7018-1 will suffice the requirement of cleints .

in some applications if your project impact reuirements are at below -46deg C you may need to choose E8018/E8018-C3 elctrodes.


Thanks & Regards,
Srinivas Rao 
welding Engineer

On Sunday, July 17, 2022 at 8:50:18 AM UTC+4 muralidharan v wrote:
Go for E 8018 electrode 

Sent from my iPhone

On 16-Jul-2022, at 6:34 PM, Kannayeram Gnanapandithan <kgpan...@gmail.com> wrote:


u have to match minimum tensile strength. in ur case, 516 gr 70 means minimum tensile is 70000psi or 485 Mpa. To match this, u can very well use 7018 which is 70000 psi or 485 Mpa. U are not supposed to match with actual tested value because it will vary. 

On Fri, Jul 15, 2022, 11:53 AM Kishore S <kishor...@gmail.com> wrote:
Dear sir 

what are the step to find an electrode for SA516 gr 70 in the internet they have mentioned E7018 but as per the SAIL TEST CERTIFICATE tensile strength is 79ksi so what electrode do I have to use   

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/ab5513fa-c564-40ce-953a-f67e68a3ea03n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/921388e9-6eb4-4b83-9bb2-1426438011dcn%40googlegroups.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...