Skip to main content

Re: [MW:31854] PWHT Requirement for Supports?

Dear

can you please provide me with a reference.
And preheat is not mentioned in WPS.

On Wed, Dec 16, 2020 at 10:21 AM 'james gerald' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Preheat to 95degC prior to welding and use multilayers to avoid PWHT for P-1 material.

Only decrease in preheat temperature greater than 55degC is an essential variable as per ASME Sec.IX and hence revise the WPS to indicate preheat min 95degC without any need for qualifying PQR and perform welding.

Thanks & Regards

J.Gerald Jayakumar




On Wednesday, 16 December, 2020, 12:38:04 pm IST, bilal wahla <bilalwahla047@gmail.com> wrote:


Dear J.Gerald  ,
Material is P-1.

On Wed, Dec 16, 2020 at 9:44 AM 'james gerald' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Generally the Pressure containing Pipe Thickness is taken as the Governing thickness when welding non-pressure part support.

But in the latest version of code there are some exceptions for some P-No's and if you could be specific it will be clear.

Thanks & Regards

J.Gerald Jayakumar




On Wednesday, 16 December, 2020, 12:04:22 pm IST, bilal wahla <bilalwahla047@gmail.com> wrote:



Greeting ALL,

On my project we are doing PWHT on Thickness basis, Pipe thickness is 30.18mm
,Will we do PWHT of Welded Supports as per B31.3? 


Bilal Arshad 
P.W.H.T QCI 

Mobile: +966 580181061

Email: bilalwahla.047@gmail.com

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMqL%2BROYYc4qzhMs9p%3Dr39KsXvUZXYe32G-CAYZ%2BBW3sj-K1wA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1030040285.867863.1608100956265%40mail.yahoo.com.


--
Respected Sir,

Please find the enclosed file.

Bilal Arshad Wahla
P.W.H.T QCI 

Mobile: +966 580181061

Email: bilalwahla.047@gmail.com

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMqL%2BRORxpTYVPeXFq%2BOqwsGndUEa-bKvBhZHyYJ-gp_Rqx2Ww%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/454718348.872505.1608103195966%40mail.yahoo.com.


--
Respected Sir,

Please find the enclosed file.

Bilal Arshad Wahla
P.W.H.T QCI 

Mobile: +966 580181061

Email: bilalwahla.047@gmail.com

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMqL%2BRNmTW-KNkfm9OjXhBzi5A6h0yFF7KXb2G3OGyGfFEkG_Q%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...