Skip to main content

Re: [MW:31825] Ferrite requirements

Dear Vengatesh,

Further to the discussion, the importance of ferrite is explained here in depth:

Duplex austenite-ferrite stainless steels should typically contain ferrite in the range 30-35 % to 60-65 % ferrite but not less than 20 or more than 70 % (approximately 30-110 FN). The phase balance is important because it determines the overall properties of the alloy: the ferrite phase imparts strength, chloride stress corrosion cracking resistance, ferromagnetic properties and solidification cracking resistance and the austenite phase imparts toughness, corrosion resistance and hydrogen cracking resistance and is non-ferromagnetic. The optimum alloy properties are achieved when the ferrite content is around 50 %. This can be achieved routinely during parent material manufacture. However, welding can change the phase balance by differing amounts, depending on the welding parameters, and so it is also important to measure the ferrite content of weld zones.

Generally, ferrite content may be measured in two basic ways: by metallographic or magnetic means. The former is usually destructive and gives results in terms of point fraction, area fraction or volume fraction (% ferrite), whereas, the latter is non-destructive and gives results in terms of a 'Ferrite Number' (FN). Unfortunately, it is not necessarily straightforward to perform, interpret and compare ferrite content measurement results, as there are several important factors which affect the results and their accuracy, for example microstructure (very important for welds), composition, size of the region examined, location of measurement, access to the region of interest and measurement method. Moreover, microstructure and composition, in particular, affect the conversion of % ferrite to FN and vice versa, which introduces uncertainties when addressing the common issue of meeting specification requirements in % ferrite when measuring a weld non-destructively using an instrument that measures FN.

MTech (Metallurgical & Materials Engineering)
Indian Institute of Technology Kharagpur (IIT)



On Thu, Dec 10, 2020 at 9:24 AM Vijay Makwana <vijaymakwana96@gmail.com> wrote:
Dear,

Duplex stainless steels are a family of corrosion-resistant alloys, which typically contain 50 % austenite and 50 % ferrite. Phase balance is important in duplex stainless steels as it helps to impart optimum mechanical properties and corrosion resistance. In many applications it is necessary to weld duplex stainless steels. Welding involves a thermal cycle that may alter the phase balance, and so it is necessary to assure that phase balance is still within acceptable ranges in the heat-affected zone and the weld metal. For example, high ferrite content may lead to lower toughness and high austenite content may lead to increased susceptibility to chloride stress corrosion cracking. Quality control of welded duplex stainless steels usually requires confirmation of an acceptable phase balance, by ferrite measurement  

Thanking you,
MTech (Metallurgical & Materials Engineering)
Indian Institute of Technology Kharagpur (IIT)



On Thu, Dec 10, 2020 at 6:34 AM Venkadesh Lakshmanan <venkadeshmech@gmail.com> wrote:
Dear Experts,

Can you please give some guidance regarding ferrite requirements for duplex stainless steel piping as per ASME B31.3. I mean what sub standards to refer, why ferrite test to be performed, either ferrite number or percentage results referring really what is in it. I understood that it is a face (bcc or fcc) , but how to describe it. Can you please give some details to know about this.

Regards,

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAA_6cSfgPMP-w7%2B7uZJsHGzQs7zjkRwqyGUgqBpn%2BEjT7YkMVw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAO96tG_V7sLPVmO6jHOV4nvub%2BmQ7UfK%2Bs4NbwFGCDczHFMU%3Dw%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...