Skip to main content

Re: [MW:31849] PWHT REQUIRED OR NOT?

Dear Ankit,

Normally Explosive Bonding will be performed at Plate Mill and any Heat Treatment if required will be performed at Mill and covered via the MTC.

SS 316 clad plates fall under SA 264 (ASME Sec.IIA). According to the same for Explosive bonding, the clad plate shall be subjected to solution Annealing and the substrate base plate carbon steel Heat Treated to the Material standard separately  prior to Explosive Bonding and can be checked in the MTC.

Thanks & Regards

J.Gerald Jayakumar




On Friday, 11 December, 2020, 03:23:16 pm IST, Patel Ankit <aapatel271@gmail.com> wrote:


Dear Sir,

Construction code ASME SEC VIII Div 1.
Explosive Bonding.

Regards,
Ankit Patel

On Tue 8 Dec, 2020, 2:15 PM 'james gerald' via Materials & Welding, <materials-welding@googlegroups.com> wrote:
Please provide below details.

1. Design Code.
2. Type of cladding like explosive cladding/cold rolling/weld metal overlay(electroslag strip/SAW strip/Laser)

Thanks & Regards

J.Gerald Jayakumar



On Tuesday, 8 December, 2020, 09:09:47 am IST, Prasad Ghanekar <prsgne@gmail.com> wrote:


Refering to SA264
HT is not mandatory for cladding process.
It's suplimentory requirement.

Prasad G.

On Mon, 7 Dec 2020, 16:58 George Dilintas, <dilintas@gmail.com> wrote:
Could you send a sketch of the joint?
You question is not clear

Στις Πέμ, 3 Δεκ 2020 στις 7:34 π.μ., ο/η udaya bhaskar <dusroni@gmail.com> έγραψε:
Hello Mr. Ankith,
Please refer  for your clarification: PART UCL REQUIREMENTS FOR WELDED PRESSURE VESSELS CONSTRUCTED OF MATERIAL WITH CORROSION RESISTANT INTEGRAL CLADDING, WELD METAL OVERLAY CLADDING, OR APPLIED LININGS 

On Wed, 2 Dec 2020, 06:12 Patel Ankit, <aapatel271@gmail.com> wrote:
Dear Expert,

I hope all are well.

My question is In after Tubesheet Bonding PWHT required or Not?

Base Material : SA 516 GR 70. (Thk : 45 mm )
Bonding Material : SA 240 GR 316. (Thk:5mm)

Tubesheet Dia : 3000 mm

( Note : Bonding plate SS 316 : 1 No joint on base material)

Regards,
Ankit Patel
8140255303.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALR-PuwRp0-NoHz6KXB6-4Y3tkTKmaB4pJxtF8HhM8ctpf3EtA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANii3RPebf2pFWS-%2BiPxoJnyobk7eWaxyqNskV1fKD4gJUEqzA%40mail.gmail.com.


--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40BHXNPTU3iqZEqGHpPuxiYd%3DyS-wS_5Tonv6ehAXyTWfw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAEi5r3bHEC%2BtYGmUM1Q6%2BNTFAwKboaO9sKyJo7eKj-Hvxj1d%2Bw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/229658807.3500830.1607401509712%40mail.yahoo.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALR-PuwWKNVJBsJ5m6yT5yR%2B6ACVDt-eoCB9-ZXV8js-oPsJQA%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .